Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Boron doped poly-Si and a-Si: Difference between revisions
Created page with "'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%http://labadviser.danchip.dtu.dk/index.php/Specific Process Knowledge/Thin ..." |
No edit summary |
||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%http://labadviser.danchip.dtu.dk/index.php/ | '''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]''' | ||
==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) == | ==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) == | ||
Revision as of 13:00, 2 November 2015
Feedback to this page: click here
Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4)
Result from Thomas Pedersen, @Nanotech, Sep 2015
Process parameters
Pressure: 250 mtorr
Temperature: 580 °C
Silane (SiH4) flow: Constant at 80 sccm
Diborane (B2H6) flow: Varied from 3 sccm to 40 sccm
Anneal: No annealing afterwards
Test wafer position: Center of the boat
Results
The Boron concentration of the film was controlled by the flow of B2H6 gas. To establish how boron doping concentration varied with B2H6 flow, films of silicon were deposited with B2H6 gas flows modulated during deposition to produce doping spikes. The two figures below show a typical SIMS concentration depth profile of a B2H6 modulation-doped film deposited on a Silicon dioxide substrate. During deposition, the gas flow of SiH4 was held constant, while flows of B2H6 was varied to create the dopant spikes.