At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system. | At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system. | ||
== Deposition of SiN with PECVD4 [[Image:section under construction.jpg|70px]] == | |||
{| border="1" cellspacing="2" cellpadding="2" | |||
|-style="background:Black; color:White" | |||
! Parameter | |||
|Recipe name: '''SiO2_res''' ('''SiO2''' etch with '''res'''ist mask) | |||
|- | |||
|Coil Power [W] | |||
|1300 | |||
|- | |||
|Platen Power [W] | |||
|200 | |||
|- | |||
|Platen temperature [<sup>o</sup>C] | |||
|0 | |||
|- | |||
|He flow [sccm] | |||
|174 | |||
|- | |||
|C<sub>4</sub>F<sub>8</sub> flow [sccm] | |||
|5 | |||
|- | |||
|H<sub>2</sub> flow [sccm] | |||
|4 | |||
|- | |||
|Pressure [mTorr] | |||
|4 | |||
|- | |||
|} | |||
{| border="2" cellspacing="2" cellpadding="3" | |||
|-style="background:DarkGray; color:White" | |||
!Material to be etched | |||
!Etch rate using SiO2_res | |||
|- | |||
|Thermal oxide | |||
| | |||
*'''~230nm/min (5% etch load)''' - etch load dependency [[/AOE SiO2 etch load dependency|'''see here''']] | |||
*~200 nm/min ''fall 2016 by Martin Lind Ommen @nanotech'' | |||
|- | |||
|TEOS oxide (5% load) | |||
|'''233nm/min ±0.7%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 ''by LN/BGE@danchip'' | |||
|- | |||
|PECVD1 (standard) oxide (5% load) | |||
|'''242nm/min ±0.6%''' - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by ''LN/BGE@danchip'' | |||
|- | |||
|Al2O3 from the ALD | |||
| | |||
*34.2 nm/min (1:6 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' | |||
*50nm can be etched in 10min - [[/Etch of Al2O3|'''See results here''']] etched in November 2014 by ''FRSTO@danchip'' | |||
|- | |||
|Silicon rich nitride from furnace B2 | |||
|136nm was etched in 1min (whole wafer) - etched in October 2015 by ''bghe@danchip'' | |||
|- | |||
|Cr | |||
|6 nm/min (1:33 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' | |||
|- | |||
|Al | |||
|25nm/min (1:8 to SiO2) ''fall 2016 by Martin Lind Ommen @nanotech'' | |||
|- | |||
|} | |||