Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD: Difference between revisions
Appearance
| Line 2: | Line 2: | ||
==Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride== | ==Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride== | ||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|NH3 flow [sccm] | |||
|N2 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|1nitride | |||
| | |||
| | |||
| | |||
| | |||
| | |||
| | |||
|- | |||
|} | |||
==Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride== | ==Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride== | ||
Revision as of 15:16, 28 November 2007
At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1nitride |
Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| MFSiNLS | 30 | 30 | 1470 | 650 | 20HF 6s
20LF 2s |
Low stress nitride - standard recipe |
| LFSiN | 30 | 15 | 1470 | 550 | 60LF | Compressive stress |
| HFSiN | 30 | 42 | 1470 | 900 | 20HF | Tensile stress |
LF=Low Frequency HF=High Frequency MF=Mixed Frequency SiN=Silicon Nitride LS=Low Stress
Expected results
| Recipe name | Deposition rate [Å/min] | RI | Uniformity [%] | Stress [MPa] |
| MFSiNLS | ~117 | ~1.99 | ~-30 | |
| LFSiN | ~550 | ~1.96 | ~3 | ~-630 |
| HFSiN | ~130 | ~1.97 | ~2 | ~460 |