| Line 62: | Line 62: | ||
|- | |- | ||
|HF SiN <!-- Recipe --> | |HF SiN <!-- Recipe --> | ||
|<!-- Dep. rate [nm/min] --> | |12.2-12.4 nm/min<!-- Dep. rate [nm/min] --> | ||
|<!-- RI --> | |2.017-2.021<!-- RI --> | ||
|<!-- Unif. [%] --> | |± 1.2-1.6%<!-- Unif. [%] --> | ||
|<!-- Stress [MPa] --> | |Tensile: 431.6 MPa<!-- Stress [MPa] --> | ||
|<!-- Comments --> | |<!-- Comments --> | ||
|<!-- SiH4 [sccm] --> | |40<!-- SiH4 [sccm] --> | ||
|<!-- NH3 [sccm] --> | |55<!-- NH3 [sccm] --> | ||
|<!-- N2O [sccm] --> | |<!-- N2O [sccm] --> | ||
|<!-- N2 [sccm] --> | |1960<!-- N2 [sccm] --> | ||
|<!-- Pressure [mTorr] --> | |900 mTorr<!-- Pressure [mTorr] --> | ||
|<!-- Power [W] --> | |20 W<!-- Power [W] --> | ||
|<!-- Load --> | |<!-- Load --> | ||
|<!-- Tune --> | |<!-- Tune --> | ||
Revision as of 08:42, 22 March 2017
Feedback to this page: click here
At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
Deposition of SiN with PECVD4 
| Recipe | Dep. rate [nm/min] | RI | Unif. [%] | Stress [MPa] | Comments | SiH4 [sccm] | NH3 [sccm] | N2O [sccm] | N2 [sccm] | Pressure [mTorr] | Power [W] | Load | Tune | Time [mm:ss] | Tested
|
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| MF SIN | 12.9-13.0 nm/min | 2.038-2.044 | ± 1.7% | 157 MPa | 40 | 40 | 1920 | 900 mTorr | 20HF6"/20LF2" | 10:00/60:00(stress) | February 2017 bghe | ||||
| LF SIN | 40-43 nm/min | 1.983-1.984 | ± 3.9-4.4% | Compressive: 565.4 MPa | 40 | 20 | 1960 | 550 mTorr | 60LF | 2:00/23:00(stress) | February 2017 bghe | ||||
| HF SiN | 12.2-12.4 nm/min | 2.017-2.021 | ± 1.2-1.6% | Tensile: 431.6 MPa | 40 | 55 | 1960 | 900 mTorr | 20 W | February 2017 bghe |
Recipes on PECVD2 for deposition of silicon nitride and silicon oxynitride
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| SINSTD80 | 30 | 20 | 1000 | 500 | 80 | |
| SINSTD96 | 30 | 20 | 1000 | 500 | 96 | |
| 1SiN | 40 | 20 | 1000 | 700 | 150 |
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] | Stress [MPa] | BHF etch rate [Å/min] | Comments |
| 1SiN |
Deposition rate in the middle of two wafers: 49nm/min+-1nm/min (2015-04-24 BGHE) |
~2-4% (2015-04-24 BGHE) |
||||
| SINSTD80 | 68nm/min (2014-07-07 JML)- unstable deposition rate | |||||
| SINSTD96 - unstable deposition rate |
Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride
| Quality Controle (QC) for PECVD3 | ||||||||||||||||||||||
|
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| MFSiNLS2 | 30 | 30 | 1470 | 845 | 100HF 7.8s
100LF 2.2s |
Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager. |
| MFSiNLS | 30 | 30 | 1470 | 650 | 20HF 6s
30LF 2s |
Low stress nitride - old standard recipe. This one is not running well any more. |
| LFSiN | 30 | 15 | 1470 | 550 | 60LF | Compressive stress |
| HFSiN | 30 | 42 | 1470 | 900 | 20HF | Tensile stress |
LF=Low Frequency HF=High Frequency MF=Mixed Frequency SiN=Silicon Nitride LS=Low Stress
Expected results
| Recipe name | Deposition rate [Å/min] | RI | Uniformity [%] [Std./mean] |
Stress [MPa] | KOH etch rate [Å/min] | BHF etch rate [Å/min] | See more |
| MFSiNLS2 | ~422 (bghe Feb 2016) | ~2.03 | ~2 | ~6 (bghe Feb 2016) | ~2.1 (bghe Feb 2016) | ~? | see DOE |
| MFSiNLS | ~107 | ~1.99 | ~4 | ~-30 | ~2.5 | ~250 | . |
| LFSiN | ~550 | ~1.96 | ~3 | ~-630 | . | . | . |
| HFSiN | ~130 | ~1.97 | ~2 | ~460 | . | . | . |
Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride. Expired!:PECVD1 has been decommissioned
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1nitride | 30 | 20 | 1000 | 500 | 80 | |
| 1nit_std | 40 | 20 | 1960 | 550 | 60 | Process control recipe |
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] | Stress [MPa] | BHF etch rate [Å/min] | Comments |
| 1nitride | ||||||
| 1nit_std | ~32 | 1.89 | ~1 | ~700 | The latest measured values can be seen in the process control sheet in LabManager |