Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/SiO2 disk and granule source tests in Temescal October 2026: Difference between revisions
Appearance
| (16 intermediate revisions by the same user not shown) | |||
| Line 9: | Line 9: | ||
Experimental work and documentation: '''Evgeniy Shkondin, DTU Nanolab'''. Rikke M. Nielsen was present during Run 1 (22 October 2026). Run 2 (23 October 2026) was carried out by Evgeniy Shkondin alone. Report updated on 27 October 2026. | Experimental work and documentation: '''Evgeniy Shkondin, DTU Nanolab'''. Rikke M. Nielsen was present during Run 1 (22 October 2026). Run 2 (23 October 2026) was carried out by Evgeniy Shkondin alone. Report updated on 27 October 2026. | ||
Service and target loading: <b>Henrik Nielsen (DTU Nanolab)</b> | |||
Photographs and schematics: Evgeniy Shkondin / DTU Nanolab. The power and rate plots are reconstructed from the instrument recordings. Both runs used a HULA (high uniformity lift-off assembly) holder; film thicknesses were determined by Cauchy-model ellipsometry. | Photographs and schematics: Evgeniy Shkondin / DTU Nanolab. The power and rate plots are reconstructed from the instrument recordings. Both runs used a HULA (high uniformity lift-off assembly) holder; film thicknesses were determined by Cauchy-model ellipsometry. | ||
| Line 40: | Line 42: | ||
|} | |} | ||
The report follows the experimental sequence using source photographs, schematics, visual observations and instrument recordings. The power curves retain the recorded values without smoothing. Run 1 heating-timer pauses are excluded from the main comparison and are separate from source instability. These exploratory tests document source | The report follows the experimental sequence using source photographs, schematics, visual observations, and instrument recordings. The power curves retain the recorded values without smoothing. Run 1 heating-timer pauses (caused by a recipe condition that issues an alarm message after 30 min of continuous heat; the value is corrected to 300 min for Run2) are excluded from the main comparison and are separate from source instability. These exploratory tests document source behavior and provide a basis for further process development. | ||
== Test design and recorded settings == | == Test design and recorded settings == | ||
| Line 56: | Line 57: | ||
|} | |} | ||
=== Common tooling-file settings === | === Common tooling-file and deposition settings === | ||
{| class="wikitable" style="width:100%;" | {| class="wikitable" style="width:100%;" | ||
| Line 67: | Line 68: | ||
| Control TC / control DT || 0.1 s / 0.1 s | | Control TC / control DT || 0.1 s / 0.1 s | ||
|- | |- | ||
| Maximum power | | Maximum allowed power || 10% | ||
|- | |||
| O<sub>2</sub> flow setting || 5% | |||
|- | |||
| Rate || 1 Å/s | |||
|- | |- | ||
| | | Thickness setpoint || 600 nm | ||
|} | |} | ||
| Line 86: | Line 91: | ||
|} | |} | ||
'''Note.''' Density is a controller input, not measured film density. O<sub>2</sub> = 5% is the instrument setting, not gas composition or partial pressure. Run 2 was reported as RT/unheated, but its logged thermocouple temperature rose from 22.0 to 61.6 °C during deposition. The TC channel is not an independent sample-surface temperature measurement. Power is recorded as percent of full scale. | '''Note.''' Density is a controller input, not measured film density. O<sub>2</sub> = 5% is the instrument setting, not gas composition or partial pressure. Run 2 was reported as RT/unheated, but its logged thermocouple temperature rose from 22.0 to 61.6 °C during deposition. The TC channel is not an independent sample-surface temperature measurement. Power is recorded as a percent of full scale. | ||
Source loading, sweep geometry and the temperature condition changed together, so this is not a single-variable comparison. The logs also show different rise/soak settings, including soak-2 levels of 2.8% in Run 1 and 5.0% in Run 2. Thickness milestones refer to the QCM indication | Source loading, sweep geometry, and the temperature condition changed together, so this is not a single-variable comparison. The logs also show different rise/soak settings, including soak-2 levels of 2.8% in Run 1 and 5.0% in Run 2. Thickness milestones refer to the QCM indication. | ||
== Run 1: solid disks alone == | == Run 1: solid disks alone == | ||
| Line 232: | Line 237: | ||
=== Implications for calibration === | === Implications for calibration === | ||
The final logged values confirm that both depositions reached the intended 600 nm range. The approximately 11% difference from ellipsometry therefore remains a calibration question | The final logged values confirm that both depositions reached the intended 600 nm range. The approximately 11% difference from ellipsometry therefore remains a calibration question (Tooling factor). | ||
The present tooling factor may be adjusted and confirmed to the different 200-mm wafer holder that differs from HULA in geometry design and wafer placement. The HULA may require a slightly higher tooling factor. | |||
== Recorded power versus thickness == | == Recorded power versus thickness == | ||
| Line 286: | Line 289: | ||
Near 587-589 nm, Run 1 recorded a rate excursion up to 7.8 Å/s while power fell to about 2.8%, followed by recovery. This occurred well after the final restart and is retained in the main curve. The log alone cannot assign it to beam repositioning, source reshaping or another specific cause. | Near 587-589 nm, Run 1 recorded a rate excursion up to 7.8 Å/s while power fell to about 2.8%, followed by recovery. This occurred well after the final restart and is retained in the main curve. The log alone cannot assign it to beam repositioning, source reshaping or another specific cause. | ||
== Processing | == Processing interpretation == | ||
[[File:Eves_SiO2_Temescal_202610_Fig09_Power_active_time.png|thumb|center|900px|Figure 9. Power plotted against cumulative time in the sustained DEPOSIT phases. Alarm pauses and conditioning are removed from the time axis. The first 120 s after each restart remain as gaps in the curve; those seconds are still part of the deposition-phase clock. This time axis differs from elapsed wall-clock time. All-phase wall-clock plots and the complete raw records are included in the accompanying package.]] | [[File:Eves_SiO2_Temescal_202610_Fig09_Power_active_time.png|thumb|center|900px|Figure 9. Power plotted against cumulative time in the sustained DEPOSIT phases. Alarm pauses (caused by a recipe condition that issues an alarm message after 30 min of continuous heat; the value is corrected to 300 min for Run2) and conditioning are removed from the time axis. The first 120 s after each restart remain as gaps in the curve; those seconds are still part of the deposition-phase clock. This time axis differs from elapsed wall-clock time. All-phase wall-clock plots and the complete raw records are included in the accompanying package.]] | ||
<div style="clear:both;"></div> | <div style="clear:both;"></div> | ||
=== Treatment of heating-timer interruptions === | === Treatment of heating-timer interruptions === | ||
Run 1 was interrupted by alarms when the 30-minute heating allowance expired. The main plots use sustained DEPOSIT phases, exclude repeated rise/soak sequences, and omit a fixed 120 s recovery interval after each restart. These exclusions are shown as gaps. Three isolated zero-power DEPOSIT-labelled records preceding restart ramps are also excluded. The initial startup is retained. | Run 1 was interrupted by alarms when the 30-minute heating allowance expired (corrected to 300 min for Run2). The main plots use sustained DEPOSIT phases, exclude repeated rise/soak sequences, and omit a fixed 120 s recovery interval after each restart. These exclusions are shown as gaps. Three isolated zero-power DEPOSIT-labelled records preceding restart ramps are also excluded. The initial startup is retained. | ||
No smoothing, outlier removal or thickness rescaling is applied to the remaining points. Original record order and small reversals in the thickness indication are preserved. The package includes the unfiltered wall-clock plots and all records. Cumulative deposition-phase time is about 101.33 min for Run 1 and 99.87 min for Run 2; the separate shutter-open counters are each 3 s shorter. | No smoothing, outlier removal or thickness rescaling is applied to the remaining points. Original record order and small reversals in the thickness indication are preserved. The package includes the unfiltered wall-clock plots and all records. Cumulative deposition-phase time is about 101.33 min for Run 1 and 99.87 min for Run 2; the separate shutter-open counters are each 3 s shorter. | ||
== Conclusions == | |||
== Conclusions | |||
=== Conclusions supported by this comparison === | === Conclusions supported by this comparison === | ||
| Line 309: | Line 306: | ||
Four solid SiO<sub>2</sub> disks alone, used with a small circular sweep, developed a cavity through the full source stack during the nominal 600 nm test. The recording captures strong early rate excursions and a late transient. The heating-timer pauses are a separate operational issue and are not evidence of source instability. The liner was reported undamaged. | Four solid SiO<sub>2</sub> disks alone, used with a small circular sweep, developed a cavity through the full source stack during the nominal 600 nm test. The recording captures strong early rate excursions and a late transient. The heating-timer pauses are a separate operational issue and are not evidence of source instability. The liner was reported undamaged. | ||
The combination of disks, surrounding granules and a horizontal figure-eight sweep gave more stable operation in the second test and left the fourth disk unpenetrated. Both configurations produced transparent SiO<sub>2</sub> films with Cauchy-model ellipsometry thicknesses close to 0.67 µm. The combined configuration is a reasonable starting point for further source optimization. | <b><em>The combination of disks, surrounding granules, and a horizontal figure-eight sweep gave more stable operation in the second test and left the fourth disk unpenetrated.</em></b> | ||
Both configurations produced transparent SiO<sub>2</sub> films with Cauchy-model ellipsometry thicknesses close to 0.67 µm. The combined configuration is a reasonable starting point for further source optimization. | |||
The strongest evidence supports improved deposition stability and reduced penetration depth in Run 2. Lower mass consumption was not quantified because the second charge was not weighed before and after deposition. A reliable maximum thickness requires further testing. | The strongest evidence supports improved deposition stability and reduced penetration depth in Run 2. Lower mass consumption was not quantified because the second charge was not weighed before and after deposition. A reliable maximum thickness requires further testing. | ||
'''Note.''' This report records exploratory tests rather than an operating instruction. Source coverage must be assessed during deposition; the absence of damage in one run does not establish that continued operation after breakthrough is acceptable. Use the current local operating procedures and tool-responsible guidance [1, 2]. | |||
=== Related local documentation === | === Related local documentation === | ||
[ | [1] DTU Nanolab LabAdviser, “Temescal processing / Good to know about the Temescal”. QCM conversion, tooling calibration and source monitoring. Accessed 27 October 2026. | ||
[https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Temescal/Good_to_know_about_the_Temescal Open the Temescal process-control guide] | [https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Temescal/Good_to_know_about_the_Temescal Open the Temescal process-control guide] | ||
[ | [2] DTU Nanolab LabAdviser, “Evaporation of SiO<sub>2</sub> in Temescal-2”. Related local process information, accessed 27 October 2026. Its earlier tests are separate from this comparison. | ||
[https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_SiO2_in_E-Beam_Evaporator_Temescal-2 Open the related SiO<sub>2</sub> deposition page] | [https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_SiO2_in_E-Beam_Evaporator_Temescal-2 Open the related SiO<sub>2</sub> deposition page] | ||