Experimental work and documentation: '''Evgeniy Shkondin, DTU Nanolab'''. Rikke M. Nielsen was present during Run 1 (22 October 2026). Run 2 (23 October 2026) was carried out by Evgeniy Shkondin alone. Report updated on 27 October 2026.
Experimental work and documentation: '''Evgeniy Shkondin, DTU Nanolab'''. Rikke M. Nielsen was present during Run 1 (22 October 2026). Run 2 (23 October 2026) was carried out by Evgeniy Shkondin alone. Report updated on 27 October 2026.
Service and target loading: <b>Henrik Nielsen (DTU Nanolab)</b>


Photographs and schematics: Evgeniy Shkondin / DTU Nanolab. The power and rate plots are reconstructed from the instrument recordings. Both runs used a HULA (high uniformity lift-off assembly) holder; film thicknesses were determined by Cauchy-model ellipsometry.
Photographs and schematics: Evgeniy Shkondin / DTU Nanolab. The power and rate plots are reconstructed from the instrument recordings. Both runs used a HULA (high uniformity lift-off assembly) holder; film thicknesses were determined by Cauchy-model ellipsometry.
Line 18: Line 20:
Two source-loading configurations were tested in the E-Beam Evaporator (10-pockets) on 22 and 23 October 2026. Each run used four solid, circular SiO<sub>2</sub> disks in a graphite liner and a nominal thickness setpoint of 600 nm at 1 Å/s. Run 1 used the disks alone. Run 2 used new disks with SiO<sub>2</sub> granules between the stack and liner wall. Both runs used a HULA (high uniformity lift-off assembly) holder.
Two source-loading configurations were tested in the E-Beam Evaporator (10-pockets) on 22 and 23 October 2026. Each run used four solid, circular SiO<sub>2</sub> disks in a graphite liner and a nominal thickness setpoint of 600 nm at 1 Å/s. Run 1 used the disks alone. Run 2 used new disks with SiO<sub>2</sub> granules between the stack and liner wall. Both runs used a HULA (high uniformity lift-off assembly) holder.


The disks alone developed a narrow cavity that penetrated the entire stack. <em>Adding granules and changing to a horizontal figure-eight sweep produced a more manageable deposition: repeated small rate spikes persisted, but the run finished without the major instability or growing liner-exposure concern</em> described for Run 1. The deepest penetration stopped at the interface between the third and fourth disks.
The disks alone developed a narrow cavity that penetrated the entire stack. <u>Adding granules and changing to a horizontal figure-eight sweep produced a more manageable deposition: repeated small rate spikes persisted, but the run finished without the major instability or growing liner-exposure concern</u> described for Run 1. The deepest penetration stopped at the interface between the third and fourth disks.


{| class="wikitable" style="width:100%;"
{| class="wikitable" style="width:100%;"
Line 40: Line 42:
|}
|}


'''Note.''' Main finding: the combined disks-and-granules configuration with sweep #7 is the more promising configuration from these two tests. Because sweep geometry and substrate temperature also changed, the improvement cannot be assigned to the granules alone.


The report follows the experimental sequence using source photographs, schematics, visual observations and instrument recordings. The power curves retain the recorded values without smoothing. Run 1 heating-timer pauses are excluded from the main comparison and are separate from source instability. These exploratory tests document source behaviour and provide a basis for further process development.
The report follows the experimental sequence using source photographs, schematics, visual observations, and instrument recordings. The power curves retain the recorded values without smoothing. Run 1 heating-timer pauses (caused by a recipe condition that issues an alarm message after 30 min of continuous heat; the value is corrected to 300 min for Run2) are excluded from the main comparison and are separate from source instability. These exploratory tests document source behavior and provide a basis for further process development.


== Test design and recorded settings ==
== Test design and recorded settings ==
Line 56: Line 57:
|}
|}


=== Common tooling-file settings ===
=== Common tooling-file and deposition settings ===


{| class="wikitable" style="width:100%;"
{| class="wikitable" style="width:100%;"
Line 67: Line 68:
| Control TC / control DT || 0.1 s / 0.1 s
| Control TC / control DT || 0.1 s / 0.1 s
|-
|-
| Maximum power / O<sub>2</sub> flow setting || 10% / 5%
| Maximum allowed power || 10%
|-
| O<sub>2</sub> flow setting || 5%
|-
| Rate || 1 Å/s
|-
|-
| Rate / thickness setpoint || 1 Å/s (0.1 nm/s) / 600 nm
| Thickness setpoint || 600 nm
|}
|}


Line 86: Line 91:
|}
|}


'''Note.''' Density is a controller input, not measured film density. O<sub>2</sub> = 5% is the instrument setting, not gas composition or partial pressure. Run 2 was reported as RT/unheated, but its logged thermocouple temperature rose from 22.0 to 61.6 °C during deposition. The TC channel is not an independent sample-surface temperature measurement. Power is recorded as percent of full scale.
'''Note.''' Density is a controller input, not measured film density. O<sub>2</sub> = 5% is the instrument setting, not gas composition or partial pressure. Run 2 was reported as RT/unheated, but its logged thermocouple temperature rose from 22.0 to 61.6 °C during deposition. The TC channel is not an independent sample-surface temperature measurement. Power is recorded as a percent of full scale.


Source loading, sweep geometry and the temperature condition changed together, so this is not a single-variable comparison. The logs also show different rise/soak settings, including soak-2 levels of 2.8% in Run 1 and 5.0% in Run 2. Thickness milestones refer to the QCM indication, not local source erosion depth. The deposition-only comparison excludes repeated conditioning in Run 1.
Source loading, sweep geometry, and the temperature condition changed together, so this is not a single-variable comparison. The logs also show different rise/soak settings, including soak-2 levels of 2.8% in Run 1 and 5.0% in Run 2. Thickness milestones refer to the QCM indication.


== Run 1: solid disks alone ==
== Run 1: solid disks alone ==
Line 232: Line 237:
=== Implications for calibration ===
=== Implications for calibration ===


The final logged values confirm that both depositions reached the intended 600 nm range. The approximately 11% difference from ellipsometry therefore remains a calibration question rather than an unrecorded extra 50 nm of indicated deposition. Relative to the post-ramp summaries, the differences are approximately +10.70% and +11.24%.
The final logged values confirm that both depositions reached the intended 600 nm range. The approximately 11% difference from ellipsometry therefore remains a calibration question (Tooling factor).  
 
The similar offsets motivate checking QCM calibration and sample position within the HULA holder before selecting a new tooling factor. QCM thickness conversion depends on density and tooling geometry [2]. The entered 2.648 g/cm<sup>3</sup> is a controller setting; the recorded thickness alone does not identify which calibration input needs adjustment.


'''Note.''' At 1 Å/s, 600 nm corresponds to 100 min. The logged shutter-open totals are consistent with this scale. Run 1’s heating-timer pauses increase elapsed time but are not included in the main comparison of deposition behaviour.
The present tooling factor may be adjusted and confirmed to the different 200-mm wafer holder that differs from HULA in geometry design and wafer placement. The HULA may require a slightly higher tooling factor.


== Recorded power versus thickness ==
== Recorded power versus thickness ==
Line 286: Line 289:
Near 587-589 nm, Run 1 recorded a rate excursion up to 7.8 Å/s while power fell to about 2.8%, followed by recovery. This occurred well after the final restart and is retained in the main curve. The log alone cannot assign it to beam repositioning, source reshaping or another specific cause.
Near 587-589 nm, Run 1 recorded a rate excursion up to 7.8 Å/s while power fell to about 2.8%, followed by recovery. This occurred well after the final restart and is retained in the main curve. The log alone cannot assign it to beam repositioning, source reshaping or another specific cause.


== Processing and physical interpretation ==
== Processing interpretation ==


[[File:Eves_SiO2_Temescal_202610_Fig09_Power_active_time.png|thumb|center|900px|Figure 9. Power plotted against cumulative time in the sustained DEPOSIT phases. Alarm pauses and conditioning are removed from the time axis. The first 120 s after each restart remain as gaps in the curve; those seconds are still part of the deposition-phase clock. This time axis differs from elapsed wall-clock time. All-phase wall-clock plots and the complete raw records are included in the accompanying package.]]
[[File:Eves_SiO2_Temescal_202610_Fig09_Power_active_time.png|thumb|center|900px|Figure 9. Power plotted against cumulative time in the sustained DEPOSIT phases. Alarm pauses (caused by a recipe condition that issues an alarm message after 30 min of continuous heat; the value is corrected to 300 min for Run2) and conditioning are removed from the time axis. The first 120 s after each restart remain as gaps in the curve; those seconds are still part of the deposition-phase clock. This time axis differs from elapsed wall-clock time. All-phase wall-clock plots and the complete raw records are included in the accompanying package.]]
<div style="clear:both;"></div>
<div style="clear:both;"></div>


=== Treatment of heating-timer interruptions ===
=== Treatment of heating-timer interruptions ===


Run 1 was interrupted by alarms when the 30-minute heating allowance expired. The main plots use sustained DEPOSIT phases, exclude repeated rise/soak sequences, and omit a fixed 120 s recovery interval after each restart. These exclusions are shown as gaps. Three isolated zero-power DEPOSIT-labelled records preceding restart ramps are also excluded. The initial startup is retained.
Run 1 was interrupted by alarms when the 30-minute heating allowance expired (corrected to 300 min for Run2). The main plots use sustained DEPOSIT phases, exclude repeated rise/soak sequences, and omit a fixed 120 s recovery interval after each restart. These exclusions are shown as gaps. Three isolated zero-power DEPOSIT-labelled records preceding restart ramps are also excluded. The initial startup is retained.


No smoothing, outlier removal or thickness rescaling is applied to the remaining points. Original record order and small reversals in the thickness indication are preserved. The package includes the unfiltered wall-clock plots and all records. Cumulative deposition-phase time is about 101.33 min for Run 1 and 99.87 min for Run 2; the separate shutter-open counters are each 3 s shorter.
No smoothing, outlier removal or thickness rescaling is applied to the remaining points. Original record order and small reversals in the thickness indication are preserved. The package includes the unfiltered wall-clock plots and all records. Cumulative deposition-phase time is about 101.33 min for Run 1 and 99.87 min for Run 2; the separate shutter-open counters are each 3 s shorter.


=== Physical interpretation remains conditional ===
== Conclusions ==
 
The narrow cavity and full-stack breakthrough in Run 1 are consistent with localized erosion under the small circular sweep. The wider figure-eight sweep and surrounding SiO<sub>2</sub> in Run 2 could distribute exposure and source reshaping more favourably. Because loading, sweep and temperature changed together, the data cannot isolate a granule effect.
 
A stable average rate can coexist with substantial cavity growth. The power trace is the controller’s response to the evolving process, not a direct source-temperature measurement. Although power and emission current are logged, a full calibrated beam-voltage history is not supplied, so energy consumption in joules is not calculated. Lower source mass consumption also remains unverified.
 
== Conclusions and next experiments ==


=== Conclusions supported by this comparison ===
=== Conclusions supported by this comparison ===
Line 309: Line 306:
Four solid SiO<sub>2</sub> disks alone, used with a small circular sweep, developed a cavity through the full source stack during the nominal 600 nm test. The recording captures strong early rate excursions and a late transient. The heating-timer pauses are a separate operational issue and are not evidence of source instability. The liner was reported undamaged.
Four solid SiO<sub>2</sub> disks alone, used with a small circular sweep, developed a cavity through the full source stack during the nominal 600 nm test. The recording captures strong early rate excursions and a late transient. The heating-timer pauses are a separate operational issue and are not evidence of source instability. The liner was reported undamaged.


The combination of disks, surrounding granules and a horizontal figure-eight sweep gave more stable operation in the second test and left the fourth disk unpenetrated. Both configurations produced transparent SiO<sub>2</sub> films with Cauchy-model ellipsometry thicknesses close to 0.67 µm. The combined configuration is a reasonable starting point for further source optimization.
<b><em>The combination of disks, surrounding granules, and a horizontal figure-eight sweep gave more stable operation in the second test and left the fourth disk unpenetrated.</em></b>
 
Both configurations produced transparent SiO<sub>2</sub> films with Cauchy-model ellipsometry thicknesses close to 0.67 µm. The combined configuration is a reasonable starting point for further source optimization.


The strongest evidence supports improved deposition stability and reduced penetration depth in Run 2. Lower mass consumption was not quantified because the second charge was not weighed before and after deposition. A reliable maximum thickness requires further testing.
The strongest evidence supports improved deposition stability and reduced penetration depth in Run 2. Lower mass consumption was not quantified because the second charge was not weighed before and after deposition. A reliable maximum thickness requires further testing.


=== Focused follow-up work ===
{| class="wikitable" style="width:100%;"
! Next step !! What it would resolve
|-
| Separate fill and sweep effects || Compare source loadings under matched temperature and a compatible fixed sweep. Then compare sweep patterns for the same loading.
|-
| Document each source loading || Retain the known disk and granulate specifications; add granulate mass, liner geometry, sweep offsets and initial source photographs.
|-
| Measure consumption consistently || Weigh the complete source charge before and after each run and account for loose fragments.
|-
| Retain and synchronize future logs || Continue saving rate, thickness, power, pressure, gas and TC channels. Add timestamps for beam shifts, source photographs and any alarms.
|-
| Repeat and characterize the films || Repeat the chosen configuration, map thickness and retain the Cauchy-model ellipsometry results. Add composition or contamination measurements if those properties determine suitability.
|}
Established practical experience in this Temescal configuration is that a granulate-only charge in a graphite liner forms a chimney - a hole through the source - when a 600 nm thickness setpoint is used, even with a figure-eight sweep. This motivated the use of solid disks together with surrounding granules.
'''Note.''' This report records exploratory tests rather than an operating instruction. Source coverage must be assessed during deposition; the absence of damage in one run does not establish that continued operation after breakthrough is acceptable. Use the current local operating procedures and tool-responsible guidance [2, 3].
== Experimental record and scope ==
=== Experimental record ===
[1] Evgeniy Shkondin, DTU Nanolab. Temescal SiO<sub>2</sub> source tests, 22-23 October 2026: experimental observations, source photographs and schematics, Cauchy-model ellipsometry results and source-mass measurements. Rikke M. Nielsen was present during Run 1; Run 2 was carried out by Evgeniy Shkondin alone.
[4] “2610229.dlg”: Run 1 instrument recording, 22 October 2026. [5] “2610234.dlg”: Run 2 instrument recording, 23 October 2026. Their dates and 6.000 kÅ / 1.0 Å/s settings match the tests. The power and rate curves are reconstructed from these files.
[6] Source-material package labels: ScoTech silicon dioxide disks, 21 mm diameter × 5 mm thick, 99.99% (4N), tracking number 2702/SiO2; Umicore Thin Film Products AG silicon dioxide granulate, 1.5-3.5 mm, 99.99%, product code 0481889. Photographs of both labels accompany the report package.
=== Setup and observation record ===


A HULA (high uniformity lift-off assembly) holder was used in both runs. The SiO<sub>2</sub> film thicknesses were obtained by Cauchy-model ellipsometry. Figure 5 records visual mental descriptions through the top chamber window, where brightness, contrast and shadowing affect interpretation. Final penetration depths were established after venting.
'''Note.''' This report records exploratory tests rather than an operating instruction. Source coverage must be assessed during deposition; the absence of damage in one run does not establish that continued operation after breakthrough is acceptable. Use the current local operating procedures and tool-responsible guidance [1, 2].


=== Related local documentation ===
=== Related local documentation ===


[2] DTU Nanolab LabAdviser, “Temescal processing / Good to know about the Temescal”. QCM conversion, tooling calibration and source monitoring. Accessed 27 October 2026.
[1] DTU Nanolab LabAdviser, “Temescal processing / Good to know about the Temescal”. QCM conversion, tooling calibration and source monitoring. Accessed 27 October 2026.


[https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Temescal/Good_to_know_about_the_Temescal Open the Temescal process-control guide]
[https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Temescal/Good_to_know_about_the_Temescal Open the Temescal process-control guide]


[3] DTU Nanolab LabAdviser, “Evaporation of SiO<sub>2</sub> in Temescal-2”. Related local process information, accessed 27 October 2026. Its earlier tests are separate from this comparison.
[2] DTU Nanolab LabAdviser, “Evaporation of SiO<sub>2</sub> in Temescal-2”. Related local process information, accessed 27 October 2026. Its earlier tests are separate from this comparison.


[https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_SiO2_in_E-Beam_Evaporator_Temescal-2 Open the related SiO<sub>2</sub> deposition page]
[https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_SiO2_in_E-Beam_Evaporator_Temescal-2 Open the related SiO<sub>2</sub> deposition page]