Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD: Difference between revisions
Appearance
| (110 intermediate revisions by 9 users not shown) | |||
| Line 1: | Line 1: | ||
{{cc-nanolab}} | |||
== | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride/Deposition_of_Silicon_Nitride_using_PECVD click here]''' <br> | ||
=== | |||
{| border="1" cellspacing=" | |||
=Deposition of Silicon Nitride using PECVD= | |||
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon nitride and silicon oxynitride. PECVD4 is for clean silicon based and III-V based samples. PECVD3 is for silicon based samples but here up 5% (4 cm2) wafer coverage of other materials as metals are allowed (under some conditions even more). Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DTU Nanolab. All though PECVD3 and PECVD4 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system. | |||
== Deposition of SiN with PECVD4 == | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD4 ''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login]<br> | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCNITRIDE=HFSIN | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|40 sccm | |||
|- | |||
|NH<sub>3</sub> flow | |||
|55 sccm | |||
|- | |- | ||
| | |N<sub>2</sub> flow | ||
|1960 sccm | |||
| | |||
|- | |- | ||
| | |Pressure | ||
| | |900 mTorr | ||
| | |- | ||
| | |RF-power | ||
| | | | ||
HF: 20 W | |||
|- | |- | ||
| | |} | ||
|40 | | align="center" valign="top"| | ||
|20 | {| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | ||
|1960 | !QC limits | ||
|550 | !PECVD4 | ||
| | |- | ||
| | |Deposition rate | ||
|11.0-13.2 nm/min | |||
|- | |||
|Non-uniformity | |||
|<3.0 % | |||
|- | |||
|Refractive Index | |||
|1.988 - 2.018 | |||
|} | |||
|- | |||
|} | |||
|} | |||
<nowiki>*</nowiki> Due to recent oscillations on the QC nitride recipe (HF), new tests were performed. Learn more about it under [[Deposition of SiN with PECVD4/NEW TESTS QC|NEW TESTS QC]] . (Still under development.) | |||
{| border="1" cellspacing="2" cellpadding="2" | |||
|-style="background:Black; color:White" | |||
!|Recipe | |||
!|Dep. rate [nm/min] | |||
!|RI | |||
!|Unif. [%] | |||
!|Stress [MPa] | |||
!|Comments | |||
!|SiH4 [sccm] | |||
!|NH3 [sccm] | |||
!|N2O [sccm] | |||
!|N2 [sccm] | |||
!|Pressure [mTorr] | |||
!|Power [W] | |||
!|Load | |||
!|Tune | |||
!|Time [mm:ss] | |||
!|Tested | |||
|- | |||
|MF SIN<!-- Recipe --> | |||
|12.9-13.0 nm/min <br> 11.7 nm/min (''kabi 2019-03-01'')<!-- Dep. rate [nm/min] --> | |||
|2.038-2.044<!-- RI --> | |||
|± 1.7%<!-- Unif. [%] --> | |||
|157 MPa <!-- Stress [MPa] --> | |||
|[[/MF_SiN results|more results]]<!-- Comments --> | |||
|40<!-- SiH4 [sccm] --> | |||
|40<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1920<!-- N2 [sccm] --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |||
|20HF6"/20LF2"<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00/60:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 Berit Herstrøm @DTU Nanolab (bghe)<!--Tested --> | |||
|- | |||
|- | |||
|MF SIN2<!-- Recipe --> | |||
|44.3 nm/min <!-- Dep. rate [nm/min] --> | |||
|2.01-2.02 <!-- RI --> | |||
|± 2.7%<!-- Unif. [%] --> | |||
|? MPa <!-- Stress [MPa] --> | |||
|<!-- Comments --> | |||
|30<!-- SiH4 [sccm] --> | |||
|30<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1470<!-- N2 [sccm] --> | |||
|850 mTorr<!-- Pressure [mTorr] --> | |||
|100HF8.2"/100LF2.2"<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00<!-- Time [mm:ss] --> | |||
|February 2020 bghe<!--Tested --> | |||
|- | |||
|LF SIN<!-- Recipe --> | |||
|40-43 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.983-1.984<!-- RI --> | |||
|± 3.9-4.4%<!-- Unif. [%] --> | |||
|Compressive: 565.4 MPa<!-- Stress [MPa] --> | |||
|<!-- Comments --> | |||
|40<!-- SiH4 [sccm] --> | |||
|20<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1960<!-- N2 [sccm] --> | |||
|550 mTorr<!-- Pressure [mTorr] --> | |||
|60LF<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|2:00/23:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |||
|HF SiN <!-- Recipe --> | |||
|12.2-12.4 nm/min<!-- Dep. rate [nm/min] --> | |||
|2.017-2.021<!-- RI --> | |||
|± 1.2-1.6%<!-- Unif. [%] --> | |||
|Tensile: 431.6 MPa<!-- Stress [MPa] --> | |||
|<!-- Comments --> | |||
|40<!-- SiH4 [sccm] --> | |||
|55<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1960<!-- N2 [sccm] --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |||
|20 W<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00/56:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |- | ||
|} | |} | ||
=== | |||
{| border="1" cellspacing=" | <br clear="all" /> | ||
<br clear="all" /> | |||
==Recipes on PECVD3 for deposition of silicon nitride== | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD3''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login]<br> | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCNITRIDE | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|30 sccm | |||
|- | |||
|NH<sub>3</sub> flow | |||
|30 sccm | |||
|- | |- | ||
| | |N<sub>2</sub> flow | ||
|1470 sccm | |||
| | |||
|- | |- | ||
| | |Pressure | ||
| | |845 mTorr | ||
| | |- | ||
| | |RF-power | ||
| | | | ||
*HF: 100 W 7.8s | |||
*LF: 100 W 2.2s | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD3 | |||
|- | |||
|Deposition rate | |||
|~40 nm/min | |||
|- | |||
|Non-uniformity | |||
|<3.0 % | |||
|- | |- | ||
| | |Refractive Index | ||
| | |2.02 - 2.04 | ||
|} | |||
| | |||
|- | |- | ||
|} | |||
|} | |} | ||
===Recipes=== | ===Recipes=== | ||
{| border="1" cellspacing="0" cellpadding="7" | {| border="1" cellspacing="0" cellpadding="7" | ||
| Line 65: | Line 218: | ||
|Power [W] | |Power [W] | ||
|Description | |Description | ||
|- | |||
|MFSiNLS2 | |||
|30 | |||
|30 | |||
|1470 | |||
|845 | |||
|100HF 7.8s | |||
100LF 2.2s | |||
|Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager. | |||
|- | |- | ||
|MFSiNLS | |MFSiNLS | ||
| Line 72: | Line 235: | ||
|650 | |650 | ||
|20HF 6s | |20HF 6s | ||
30LF 2s | |||
|Low stress nitride - standard recipe | |Low stress nitride - old standard recipe. This one is not running well any more. | ||
|- | |- | ||
|LFSiN | |LFSiN | ||
| Line 102: | Line 265: | ||
|Uniformity [%]<br \>[Std./mean] | |Uniformity [%]<br \>[Std./mean] | ||
|Stress [MPa] | |Stress [MPa] | ||
|KOH etch rate [Å/min] | |||
|BHF etch rate [Å/min] | |||
|See more | |||
|- | |- | ||
|MFSiNLS2 | |||
|~422 (''bghe Feb 2016'') | |||
|~2.03 | |||
|~2 | |||
|~6 (''bghe Feb 2016'') | |||
|~2.1 (''bghe Feb 2016'') | |||
|~? | |||
|[[/PECVD3: Low stress nitride testing|see more results]] | |||
|- | |||
|MFSiNLS | |MFSiNLS | ||
|~ | |~107 | ||
|~1.99 | |~1.99 | ||
|~4 | |~4 | ||
|~-30 | |~-30 | ||
|~2.5 | |||
|~250 | |||
|. | |||
|- | |- | ||
|LFSiN | |LFSiN | ||
| Line 114: | Line 292: | ||
|~3 | |~3 | ||
|~-630 | |~-630 | ||
|. | |||
|. | |||
|. | |||
|- | |- | ||
|HFSiN | |HFSiN | ||
| Line 120: | Line 301: | ||
|~2 | |~2 | ||
|~460 | |~460 | ||
|. | |||
|. | |||
|. | |||
|- | |- | ||
|} | |} | ||
==Recipes on PECVD2 for Deposition of Silicon Nitride== | |||
'''<span style="color:Red">Expired Recipes! The PECVD2 has been decomissioned and is no longer available.</span>''' | |||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|NH3 flow [sccm] | |||
|N2 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|SINSTD80 | |||
|30 | |||
|20 | |||
|1000 | |||
|500 | |||
|80 | |||
| | |||
|- | |||
|SINSTD96 | |||
|30 | |||
|20 | |||
|1000 | |||
|500 | |||
|96 | |||
| | |||
|- | |||
|1SiN | |||
|40 | |||
|20 | |||
|1000 | |||
|700 | |||
|150 | |||
| | |||
|- | |||
|} | |||
===Expected results=== | |||
{| border="1" cellspacing="0" cellpadding="5" | |||
|- | |||
|Recipe name | |||
|Deposition rate [nm/min] | |||
|RI | |||
|Uniformity [%] | |||
|Stress [MPa] | |||
|BHF etch rate [Å/min] | |||
|Comments | |||
|- | |||
|1SiN | |||
| | |||
Deposition rate in the middle of two wafers: '''49nm/min+-1nm/min''' (2015-04-24 BGHE) <br> | |||
In the middel: '''72.6-76.4 nm/min''' (2014-08-13 BGHE) ''Old shower head''<br> | |||
Variation over 3 wafers: '''71.4-78.6 nm/min''' (2014-08-13 BGHE) ''Old shower head'' | |||
| | |||
| | |||
'''~2-4%''' (2015-04-24 BGHE)<br> | |||
'''~5%''' in the middel (4") (2014-08-13 BGHE) ''Old shower head''<br> | |||
'''~10%''' over 3 wafers (2014-08-13 BGHE) ''Old shower head'' | |||
| | |||
| | |||
| | |||
|- | |||
|SINSTD80 | |||
|68nm/min (2014-07-07 JML)- unstable deposition rate | |||
| | |||
| | |||
| | |||
| | |||
| | |||
|- | |||
|SINSTD96 - unstable deposition rate | |||
| | |||
| | |||
| | |||
| | |||
| | |||
| | |||
|- | |||
|} | |||
==Recipes on PECVD1 for Deposition of Silicon Nitride== | |||
'''<span style="color:Red">Expired Recipes! The PECVD1 has been decomissioned and is no longer available.</span>''' | |||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|NH3 flow [sccm] | |||
|N2 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|1nitride | |||
|30 | |||
|20 | |||
|1000 | |||
|500 | |||
|80 | |||
| | |||
|- | |||
|1nit_std | |||
|40 | |||
|20 | |||
|1960 | |||
|550 | |||
|60 | |||
|Process control recipe | |||
|- | |||
|} | |||
===Expected results=== | |||
{| border="1" cellspacing="0" cellpadding="5" | |||
|- | |||
|Recipe name | |||
|Deposition rate [nm/min] | |||
|RI | |||
|Uniformity [%] | |||
|Stress [MPa] | |||
|BHF etch rate [Å/min] | |||
|Comments | |||
|- | |||
|1nitride | |||
| | |||
| | |||
| | |||
| | |||
| | |||
| | |||
|- | |||
|1nit_std | |||
|~32 | |||
|1.89 | |||
|~1 | |||
| | |||
|~700 | |||
|The latest measured values can be seen in the process control sheet in LabManager | |||
|- | |||
|} | |||
=Oxynitrides= | |||
The recipe for making oxynitrides will depend on what kind of oxynitride you need. If you need a little higher refractive index than SiO2 then start with an SiO2 recipe and then add NH3 until the right refractive index is obtained. If you need very high refractive index a little lower than for silicon nitride then it is probably better to start with a silicon nitride recipe and add a some N2O until you get the right refractive index. | |||
We had a Ph.d student long time ago Klaus Bo Mogensen that did the first. You can find his ph.d. thesis here: [https://findit.dtu.dk/en/catalog?author=Mogensen&q=title%3A%28Integration+of+Planar+Waveguides+for+Optical+Detection+in+Microfabricated+Analytical+Devices%29 Integration of Planar Waveguides for Optical Detection in Microfabricated Analytical Devices] | |||
Berit H. has the thesis in her office. | |||