Jump to content

Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Boron doped poly-Si and a-Si: Difference between revisions

Kabi (talk | contribs)
No edit summary
Mmat (talk | contribs)
mNo edit summary
 
(13 intermediate revisions by 3 users not shown)
Line 1: Line 1:
{{cc-nanolab}}
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]'''


==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
''Result from Thomas Pedersen, @Nanotech, Sep 2015''
''Result from Thomas Pedersen, DTU Nanotech (now DTU Nanolab), September 2015''
====Process parameters====
====Process parameters====


Line 31: Line 34:
[[image:Boron concentration2.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.]]
[[image:Boron concentration2.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.]]


'''
<br clear="all" />


== Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
== Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
Line 37: Line 40:


====Process parameters====
====Process parameters====
The test was made on a n-type silicon wafer (100) with a 110 nm grown thermal oxide)


'''Pressure:'''  250 mtorr
'''Pressure:'''  250 mtorr
Line 48: Line 52:
'''Time:''' 75 min
'''Time:''' 75 min


'''Anneal:''' @950°C for 60 min
'''Anneal:''' @950°C for 60 min in N<sub>2</sub>


'''Test wafer position:''' Center of the boat
'''Test wafer position:''' Center of the boat
A better uniformity of the resistivity across the wafer was achieved by subsequently annealing in N<sub>2</sub>, the annealing was done in Anneal Oxide Furnace (C1). The measured film thickness was 370 nm and the sheet resistance was measured to 200 &Omega;/sq +/- 15 &Omega;/sq.