Jump to content

Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Boron doped poly-Si and a-Si: Difference between revisions

Paphol (talk | contribs)
Created page with "'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%http://labadviser.danchip.dtu.dk/index.php/Specific Process Knowledge/Thin ..."
 
Mmat (talk | contribs)
mNo edit summary
 
(19 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%http://labadviser.danchip.dtu.dk/index.php/Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Boron doped poly-Si and a-Si click here]'''
{{cc-nanolab}}
 
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]'''
 


==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
''Result from Thomas Pedersen, @Nanotech, Sep 2015''
''Result from Thomas Pedersen, DTU Nanotech (now DTU Nanolab), September 2015''
====Process parameters====
====Process parameters====


Line 30: Line 33:


[[image:Boron concentration2.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.]]
[[image:Boron concentration2.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.]]
<br clear="all" />
== Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
''Result from Trine Holm Christensen, @Space, Feb. 2015''
====Process parameters====
The test was made on a n-type silicon wafer (100) with a 110 nm grown thermal oxide)
'''Pressure:'''  250 mtorr
'''Temperature:''' 580 °C
'''Silane (SiH<sub>4</sub>) flow:''' 80 sccm
'''Diborane (B<sub>2</sub>H<sub>6</sub>) flow:''' 7 sccm
'''Time:''' 75 min
'''Anneal:''' @950°C for 60 min in N<sub>2</sub>
'''Test wafer position:''' Center of the boat
A better uniformity of the resistivity across the wafer was achieved by subsequently annealing in N<sub>2</sub>, the annealing was done in Anneal Oxide Furnace (C1). The measured film thickness was 370 nm and the sheet resistance was measured to 200 &Omega;/sq +/- 15 &Omega;/sq.