Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of Silicon Nitride using PECVD: Difference between revisions
| (116 intermediate revisions by 10 users not shown) | |||
| Line 1: | Line 1: | ||
{{cc-nanolab}} | |||
= | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride/Deposition_of_Silicon_Nitride_using_PECVD click here]''' <br> | ||
==Recipes on PECVD3 for deposition of silicon nitride | =Deposition of Silicon Nitride using PECVD= | ||
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon nitride and silicon oxynitride. PECVD4 is for clean silicon based and III-V based samples. PECVD3 is for silicon based samples but here up 5% (4 cm2) wafer coverage of other materials as metals are allowed (under some conditions even more). Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DTU Nanolab. All though PECVD3 and PECVD4 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system. | |||
== Deposition of SiN with PECVD4 == | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD4 ''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login]<br> | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCNITRIDE=HFSIN | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|40 sccm | |||
|- | |||
|NH<sub>3</sub> flow | |||
|55 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|1960 sccm | |||
|- | |||
|Pressure | |||
|900 mTorr | |||
|- | |||
|RF-power | |||
| | |||
HF: 20 W | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD4 | |||
|- | |||
|Deposition rate | |||
|11.0-13.2 nm/min | |||
|- | |||
|Non-uniformity | |||
|<3.0 % | |||
|- | |||
|Refractive Index | |||
|1.988 - 2.018 | |||
|} | |||
|- | |||
|} | |||
|} | |||
<nowiki>*</nowiki> Due to recent oscillations on the QC nitride recipe (HF), new tests were performed. Learn more about it under [[Deposition of SiN with PECVD4/NEW TESTS QC|NEW TESTS QC]] . (Still under development.) | |||
{| border="1" cellspacing="2" cellpadding="2" | |||
|-style="background:Black; color:White" | |||
!|Recipe | |||
!|Dep. rate [nm/min] | |||
!|RI | |||
!|Unif. [%] | |||
!|Stress [MPa] | |||
!|Comments | |||
!|SiH4 [sccm] | |||
!|NH3 [sccm] | |||
!|N2O [sccm] | |||
!|N2 [sccm] | |||
!|Pressure [mTorr] | |||
!|Power [W] | |||
!|Load | |||
!|Tune | |||
!|Time [mm:ss] | |||
!|Tested | |||
|- | |||
|MF SIN<!-- Recipe --> | |||
|12.9-13.0 nm/min <br> 11.7 nm/min (''kabi 2019-03-01'')<!-- Dep. rate [nm/min] --> | |||
|2.038-2.044<!-- RI --> | |||
|± 1.7%<!-- Unif. [%] --> | |||
|157 MPa <!-- Stress [MPa] --> | |||
|[[/MF_SiN results|more results]]<!-- Comments --> | |||
|40<!-- SiH4 [sccm] --> | |||
|40<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1920<!-- N2 [sccm] --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |||
|20HF6"/20LF2"<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00/60:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 Berit Herstrøm @DTU Nanolab (bghe)<!--Tested --> | |||
|- | |||
|- | |||
|MF SIN2<!-- Recipe --> | |||
|44.3 nm/min <!-- Dep. rate [nm/min] --> | |||
|2.01-2.02 <!-- RI --> | |||
|± 2.7%<!-- Unif. [%] --> | |||
|? MPa <!-- Stress [MPa] --> | |||
|<!-- Comments --> | |||
|30<!-- SiH4 [sccm] --> | |||
|30<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1470<!-- N2 [sccm] --> | |||
|850 mTorr<!-- Pressure [mTorr] --> | |||
|100HF8.2"/100LF2.2"<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00<!-- Time [mm:ss] --> | |||
|February 2020 bghe<!--Tested --> | |||
|- | |||
|LF SIN<!-- Recipe --> | |||
|40-43 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.983-1.984<!-- RI --> | |||
|± 3.9-4.4%<!-- Unif. [%] --> | |||
|Compressive: 565.4 MPa<!-- Stress [MPa] --> | |||
|<!-- Comments --> | |||
|40<!-- SiH4 [sccm] --> | |||
|20<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1960<!-- N2 [sccm] --> | |||
|550 mTorr<!-- Pressure [mTorr] --> | |||
|60LF<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|2:00/23:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |||
|HF SiN <!-- Recipe --> | |||
|12.2-12.4 nm/min<!-- Dep. rate [nm/min] --> | |||
|2.017-2.021<!-- RI --> | |||
|± 1.2-1.6%<!-- Unif. [%] --> | |||
|Tensile: 431.6 MPa<!-- Stress [MPa] --> | |||
|<!-- Comments --> | |||
|40<!-- SiH4 [sccm] --> | |||
|55<!-- NH3 [sccm] --> | |||
|<!-- N2O [sccm] --> | |||
|1960<!-- N2 [sccm] --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |||
|20 W<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00/56:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |||
|} | |||
<br clear="all" /> | |||
<br clear="all" /> | |||
==Recipes on PECVD3 for deposition of silicon nitride== | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD3''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login]<br> | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCNITRIDE | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|30 sccm | |||
|- | |||
|NH<sub>3</sub> flow | |||
|30 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|1470 sccm | |||
|- | |||
|Pressure | |||
|845 mTorr | |||
|- | |||
|RF-power | |||
| | |||
*HF: 100 W 7.8s | |||
*LF: 100 W 2.2s | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD3 | |||
|- | |||
|Deposition rate | |||
|~40 nm/min | |||
|- | |||
|Non-uniformity | |||
|<3.0 % | |||
|- | |||
|Refractive Index | |||
|2.02 - 2.04 | |||
|} | |||
|- | |||
|} | |||
|} | |||
===Recipes=== | ===Recipes=== | ||
{| border="1" cellspacing="0" cellpadding="7" | {| border="1" cellspacing="0" cellpadding="7" | ||
| Line 15: | Line 218: | ||
|Power [W] | |Power [W] | ||
|Description | |Description | ||
|- | |||
|MFSiNLS2 | |||
|30 | |||
|30 | |||
|1470 | |||
|845 | |||
|100HF 7.8s | |||
100LF 2.2s | |||
|Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager. | |||
|- | |- | ||
|MFSiNLS | |MFSiNLS | ||
| Line 22: | Line 235: | ||
|650 | |650 | ||
|20HF 6s | |20HF 6s | ||
30LF 2s | |||
|Low stress nitride - standard recipe | |Low stress nitride - old standard recipe. This one is not running well any more. | ||
|- | |- | ||
|LFSiN | |LFSiN | ||
| Line 50: | Line 263: | ||
|Deposition rate [Å/min] | |Deposition rate [Å/min] | ||
|RI | |RI | ||
|Uniformity [%] | |Uniformity [%]<br \>[Std./mean] | ||
|Stress [MPa] | |Stress [MPa] | ||
|KOH etch rate [Å/min] | |||
|BHF etch rate [Å/min] | |||
|See more | |||
|- | |- | ||
|MFSiNLS2 | |||
|~422 (''bghe Feb 2016'') | |||
|~2.03 | |||
|~2 | |||
|~6 (''bghe Feb 2016'') | |||
|~2.1 (''bghe Feb 2016'') | |||
|~? | |||
|[[/PECVD3: Low stress nitride testing|see more results]] | |||
|- | |||
|MFSiNLS | |MFSiNLS | ||
|~ | |~107 | ||
|~1.99 | |~1.99 | ||
| | |~4 | ||
|~-30 | |~-30 | ||
|~2.5 | |||
|~250 | |||
|. | |||
|- | |- | ||
|LFSiN | |LFSiN | ||
| Line 64: | Line 292: | ||
|~3 | |~3 | ||
|~-630 | |~-630 | ||
|. | |||
|. | |||
|. | |||
|- | |- | ||
|HFSiN | |HFSiN | ||
| Line 70: | Line 301: | ||
|~2 | |~2 | ||
|~460 | |~460 | ||
|. | |||
|. | |||
|. | |||
|- | |- | ||
|} | |} | ||
==Recipes on PECVD2 for Deposition of Silicon Nitride== | |||
'''<span style="color:Red">Expired Recipes! The PECVD2 has been decomissioned and is no longer available.</span>''' | |||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|NH3 flow [sccm] | |||
|N2 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|SINSTD80 | |||
|30 | |||
|20 | |||
|1000 | |||
|500 | |||
|80 | |||
| | |||
|- | |||
|SINSTD96 | |||
|30 | |||
|20 | |||
|1000 | |||
|500 | |||
|96 | |||
| | |||
|- | |||
|1SiN | |||
|40 | |||
|20 | |||
|1000 | |||
|700 | |||
|150 | |||
| | |||
|- | |||
|} | |||
===Expected results=== | |||
{| border="1" cellspacing="0" cellpadding="5" | |||
|- | |||
|Recipe name | |||
|Deposition rate [nm/min] | |||
|RI | |||
|Uniformity [%] | |||
|Stress [MPa] | |||
|BHF etch rate [Å/min] | |||
|Comments | |||
|- | |||
|1SiN | |||
| | |||
Deposition rate in the middle of two wafers: '''49nm/min+-1nm/min''' (2015-04-24 BGHE) <br> | |||
In the middel: '''72.6-76.4 nm/min''' (2014-08-13 BGHE) ''Old shower head''<br> | |||
Variation over 3 wafers: '''71.4-78.6 nm/min''' (2014-08-13 BGHE) ''Old shower head'' | |||
| | |||
| | |||
'''~2-4%''' (2015-04-24 BGHE)<br> | |||
'''~5%''' in the middel (4") (2014-08-13 BGHE) ''Old shower head''<br> | |||
'''~10%''' over 3 wafers (2014-08-13 BGHE) ''Old shower head'' | |||
| | |||
| | |||
| | |||
|- | |||
|SINSTD80 | |||
|68nm/min (2014-07-07 JML)- unstable deposition rate | |||
| | |||
| | |||
| | |||
| | |||
| | |||
|- | |||
|SINSTD96 - unstable deposition rate | |||
| | |||
| | |||
| | |||
| | |||
| | |||
| | |||
|- | |||
|} | |||
==Recipes on PECVD1 for Deposition of Silicon Nitride== | |||
'''<span style="color:Red">Expired Recipes! The PECVD1 has been decomissioned and is no longer available.</span>''' | |||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|NH3 flow [sccm] | |||
|N2 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|1nitride | |||
|30 | |||
|20 | |||
|1000 | |||
|500 | |||
|80 | |||
| | |||
|- | |||
|1nit_std | |||
|40 | |||
|20 | |||
|1960 | |||
|550 | |||
|60 | |||
|Process control recipe | |||
|- | |||
|} | |||
===Expected results=== | |||
{| border="1" cellspacing="0" cellpadding="5" | |||
|- | |||
|Recipe name | |||
|Deposition rate [nm/min] | |||
|RI | |||
|Uniformity [%] | |||
|Stress [MPa] | |||
|BHF etch rate [Å/min] | |||
|Comments | |||
|- | |||
|1nitride | |||
| | |||
| | |||
| | |||
| | |||
| | |||
| | |||
|- | |||
|1nit_std | |||
|~32 | |||
|1.89 | |||
|~1 | |||
| | |||
|~700 | |||
|The latest measured values can be seen in the process control sheet in LabManager | |||
|- | |||
|} | |||
=Oxynitrides= | |||
The recipe for making oxynitrides will depend on what kind of oxynitride you need. If you need a little higher refractive index than SiO2 then start with an SiO2 recipe and then add NH3 until the right refractive index is obtained. If you need very high refractive index a little lower than for silicon nitride then it is probably better to start with a silicon nitride recipe and add a some N2O until you get the right refractive index. | |||
We had a Ph.d student long time ago Klaus Bo Mogensen that did the first. You can find his ph.d. thesis here: [https://findit.dtu.dk/en/catalog?author=Mogensen&q=title%3A%28Integration+of+Planar+Waveguides+for+Optical+Detection+in+Microfabricated+Analytical+Devices%29 Integration of Planar Waveguides for Optical Detection in Microfabricated Analytical Devices] | |||
Berit H. has the thesis in her office. | |||
Latest revision as of 10:23, 30 October 2025
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Deposition of Silicon Nitride using PECVD
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon nitride and silicon oxynitride. PECVD4 is for clean silicon based and III-V based samples. PECVD3 is for silicon based samples but here up 5% (4 cm2) wafer coverage of other materials as metals are allowed (under some conditions even more). Look at the PECVD page to learn more about the PECVDs at DTU Nanolab. All though PECVD3 and PECVD4 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
Deposition of SiN with PECVD4
| Quality Control (QC) for PECVD4 | ||||||||||||||||||||||
|
* Due to recent oscillations on the QC nitride recipe (HF), new tests were performed. Learn more about it under NEW TESTS QC . (Still under development.)
| Recipe | Dep. rate [nm/min] | RI | Unif. [%] | Stress [MPa] | Comments | SiH4 [sccm] | NH3 [sccm] | N2O [sccm] | N2 [sccm] | Pressure [mTorr] | Power [W] | Load | Tune | Time [mm:ss] | Tested
|
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| MF SIN | 12.9-13.0 nm/min 11.7 nm/min (kabi 2019-03-01) |
2.038-2.044 | ± 1.7% | 157 MPa | more results | 40 | 40 | 1920 | 900 mTorr | 20HF6"/20LF2" | 10:00/60:00(stress) | February 2017 Berit Herstrøm @DTU Nanolab (bghe) | |||
| MF SIN2 | 44.3 nm/min | 2.01-2.02 | ± 2.7% | ? MPa | 30 | 30 | 1470 | 850 mTorr | 100HF8.2"/100LF2.2" | 10:00 | February 2020 bghe | ||||
| LF SIN | 40-43 nm/min | 1.983-1.984 | ± 3.9-4.4% | Compressive: 565.4 MPa | 40 | 20 | 1960 | 550 mTorr | 60LF | 2:00/23:00(stress) | February 2017 bghe | ||||
| HF SiN | 12.2-12.4 nm/min | 2.017-2.021 | ± 1.2-1.6% | Tensile: 431.6 MPa | 40 | 55 | 1960 | 900 mTorr | 20 W | 10:00/56:00(stress) | February 2017 bghe |
Recipes on PECVD3 for deposition of silicon nitride
| Quality Controle (QC) for PECVD3 | ||||||||||||||||||||||
|
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| MFSiNLS2 | 30 | 30 | 1470 | 845 | 100HF 7.8s
100LF 2.2s |
Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager. |
| MFSiNLS | 30 | 30 | 1470 | 650 | 20HF 6s
30LF 2s |
Low stress nitride - old standard recipe. This one is not running well any more. |
| LFSiN | 30 | 15 | 1470 | 550 | 60LF | Compressive stress |
| HFSiN | 30 | 42 | 1470 | 900 | 20HF | Tensile stress |
LF=Low Frequency HF=High Frequency MF=Mixed Frequency SiN=Silicon Nitride LS=Low Stress
Expected results
| Recipe name | Deposition rate [Å/min] | RI | Uniformity [%] [Std./mean] |
Stress [MPa] | KOH etch rate [Å/min] | BHF etch rate [Å/min] | See more |
| MFSiNLS2 | ~422 (bghe Feb 2016) | ~2.03 | ~2 | ~6 (bghe Feb 2016) | ~2.1 (bghe Feb 2016) | ~? | see more results |
| MFSiNLS | ~107 | ~1.99 | ~4 | ~-30 | ~2.5 | ~250 | . |
| LFSiN | ~550 | ~1.96 | ~3 | ~-630 | . | . | . |
| HFSiN | ~130 | ~1.97 | ~2 | ~460 | . | . | . |
Recipes on PECVD2 for Deposition of Silicon Nitride
Expired Recipes! The PECVD2 has been decomissioned and is no longer available.
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| SINSTD80 | 30 | 20 | 1000 | 500 | 80 | |
| SINSTD96 | 30 | 20 | 1000 | 500 | 96 | |
| 1SiN | 40 | 20 | 1000 | 700 | 150 |
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] | Stress [MPa] | BHF etch rate [Å/min] | Comments |
| 1SiN |
Deposition rate in the middle of two wafers: 49nm/min+-1nm/min (2015-04-24 BGHE) |
~2-4% (2015-04-24 BGHE) |
||||
| SINSTD80 | 68nm/min (2014-07-07 JML)- unstable deposition rate | |||||
| SINSTD96 - unstable deposition rate |
Recipes on PECVD1 for Deposition of Silicon Nitride
Expired Recipes! The PECVD1 has been decomissioned and is no longer available.
Recipes
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1nitride | 30 | 20 | 1000 | 500 | 80 | |
| 1nit_std | 40 | 20 | 1960 | 550 | 60 | Process control recipe |
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] | Stress [MPa] | BHF etch rate [Å/min] | Comments |
| 1nitride | ||||||
| 1nit_std | ~32 | 1.89 | ~1 | ~700 | The latest measured values can be seen in the process control sheet in LabManager |
Oxynitrides
The recipe for making oxynitrides will depend on what kind of oxynitride you need. If you need a little higher refractive index than SiO2 then start with an SiO2 recipe and then add NH3 until the right refractive index is obtained. If you need very high refractive index a little lower than for silicon nitride then it is probably better to start with a silicon nitride recipe and add a some N2O until you get the right refractive index.
We had a Ph.d student long time ago Klaus Bo Mogensen that did the first. You can find his ph.d. thesis here: Integration of Planar Waveguides for Optical Detection in Microfabricated Analytical Devices
Berit H. has the thesis in her office.