Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using LPCVD TEOS: Difference between revisions

From LabAdviser
Rkc (talk | contribs)
No edit summary
Pevo (talk | contribs)
 
(62 intermediate revisions by 5 users not shown)
Line 1: Line 1:
TEOS oxide, has a dielectric
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_LPCVD_TEOS click here]'''
constant of 3.56 (For thermal oxide it is 3.46). Furthermore TEOS has a breakdown
voltage in the order of <math> 10^6 </math>


Danchip have two [[Specific Process Knowledge/Thin film deposition/B2 Furnace LPCVD Nitride|LPCVD furnaces]] for deposition of silicon nitride: A new furnace (installed in 2008) for deposition of stoichiometric nitride on 4" and 6" wafers and an older furnace (installed in 1995) for deposition of stoichiometric nitride and low stress nitride on 4" wafers. Please, be aware that it is not allowed to deposit low stress nitride i the new nitride furnace (to avoid problems with particles).
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i>


On the new LPCVD nitride furnace there are two standard processes for deposition of stoichiometric nitride, one for 4" wafers called "4NITDAN" and one for 6" wafers called "6NITDAN". The old LPCVD nitride furnace is mainly dedicated for deposition of low stress nitride, which does affect the cleanliness of the furnace, but stoichiometric nitride can also be deposited in the furnace. On this furnace the process for stoichiometric nitride is called "NITRIDE", and the process for low stress nitride (silicon rich nitride) is called "SIRICH"
==LPCVD TEOS oxide deposition==


==Process parameters for the two standard deposition recipes on the old nitride furnace:==
[[Image:teos1.jpg|300x300px|thumb|Figure 1: TEOS molecule structure]]
{| border="2" cellspacing="1" cellpadding="5"
[[Image:TEOS.jpg|300x300px|thumb|Figure 2: LPCVD TEOS oxide deposited on Si trenches]]
!Recipe name
!Wafer size and number of wafers
!Temperature [<sup>o</sup>C]
!Pressure [mTorr]
!NH3 gas flow [sccm]
!DCS gas flow [sccm]
!Comments
|-
|"NITRIDE"
|4" wafers
1-35 wafers in a run
|800 - 825
|230
|75
|25
|Stoichiometric nitride
|-
|"SIRICH"
|4" wafers
1-35 wafers in a run
|835
|112
|13
|93
|Low stress nitride (silicon rich nitride)


This was first tested at DTU Danchip by Matthias Heschel,<br \> ''M. Heschel and S. Bouwstra "Robust, compliant silicon nitride membranes", Proceedings MME '95, Copenhagen, Denmark, September 1995, pp. 84-87''
DTU Nanolab has one furnace for deposition of LPCVD TEOS oxide. The furnace is a Tempress horizontal furnace, and it was installed in the cleanroom in 1995.
|}


==Expected results when using the two standard recipes on the old nitride furnace:==
In the furnace LPCVD TEOS oxide can be deposited on up to 15 4" wafers. It is not possible to deposit TEOS oxide on 6" wafers in he cleanroom.  
These are typical values
{| border="2" cellspacing="1" cellpadding="6"
!Recipe name
!Deposition rate [Å/min]
!Refractive index@630nm
!Thickness variation on wafer
!Thickness variation along the boat
!Stress [MPa]
|-
|"NITRIDE"
|46-52
|2.01-2.02
|<1.3%
|<4%
|1000
|-
|"SIRICH"
|30-40
|2.20-2.30
|<5%
|<20%
|(-50 to 50)
|-
|}


==Process parameters for the two standard deposition recipes on the new nitride furnace:==
TEOS is is Tetra-Ethyl-Ortho-Silicate, sometimes also referred to as Tetra-Ethoxy-Silane, and it has the chemical formula Si(C<sub>2</sub>H<sub>5</sub>O)<sub>4</sub>. The molecular structure can be seen figure 1. It is a liquid that is stored in a bubbler. When a deposition is started, the bubbler is heated to 75 <sup>o</sup>C, and TEOS is then vaporized and introduced into the furnace. The TEOS flow is controlled by an MFC (mass flow controller).
{| border="2" cellspacing="1" cellpadding="5"
!Recipe name
!Wafer size and number of wafers
!Temperature [<sup>o</sup>C]
!Pressure [mTorr]
!NH3 gas flow [sccm]
!DCS gas flow [sccm]
!Comments
|-
|"4NITDAN"
|4" wafers
1-25 wafers in a run
|780 - 790
|200
|100
|33
|Stoichiometric nitride
|-
|"6NITDAN"
|6" wafers
1-25 wafers in a run
|780 - 790
|200
|120
|30
|Stoichiometric nitride
|}


==Expected results when using the two standard recipes on the new nitride furnace:==
In the furnace, TEOS is thermally decomposed on the sample surface, so that a layer of silicon dioxide (SiO<sub>2</sub>) is deposited there:
These are typical values
{| border="2" cellspacing="1" cellpadding="6"
!Recipe name
!Deposition rate [Å/min]
!Refractive index@630nm
!Thickness variation on wafer
!Thickness variation along the boat
!Stress [MPa]
|-
|"4NITDAN"
|~ 30-35
|2.00 - 2.01
|<3%
|<3%
|
|-
|"6NITDAN"
|~ 30-35
|2.00 - 2.01
|<3%
|
|-
|}


==Using LPCVD silicon nitride as a masking material for KOH etching==
Si(C<sub>2</sub>H<sub>5</sub>O)<sub>4</sub> ''(l)'' → SiO<sub>2</sub> ''(s)'' + 4 CH<sub>2</sub>H<sub>4</sub> ''(g)'' + 2 H<sub>2</sub>O ''(g)''
At Danchip stoichiometric silicon nitride is mainly used as masking material for potassium hydroxide (KOH) etching. The etch rate of the nitride in 80 <sup>o</sup>C KOH is expected to be less than 1 Å/min.


There are regularly users having problems with pinholes in the silicon nitride after KOH etching. It is not always clear what the reasons are, but we suspect problems can arise due to
Carbon can be incorporated in the TEOS oxide layer, but this can be reduced by an annealing - see below.  
*too many or too large particles in the nitride.
*too rough handling of the wafers after the nitride deposition.
*too much stress between the nitride and the underlying layer.


The difference between TEOS and silane gas (used for deposition of silicon nitride) is essentially that in TEOS the silicon atom is already oxidized. Therefore the conversion of TEOS to silicon dioxide is a rearrangement rather than an oxidation. As can be seen from figure 1 what is basically required to deposit silicon dioxide is a removal of two oxygen atoms, and for that to happen a relative high temperature of 720 <sup>o</sup>C is needed.   


===Our recommendations to try and avoid pinhole problems are:===
TEOS molecules have a very high surface mobility enabling the TEOS oxide to fill holes that have a large aspect ratio and leaving the surface quite smooth, see figure 2, hence it also covers corners and side walls very well. However very small nanometer trenched and/or very deep trenches will be challenging to fill.
'''To avoid too many or too large particles in the nitride'''<br\>
*Use the new nitride furnace, if you have to deposit stoichiometric nitride. In order to avoid problems with particles it is not allowed to deposit low stress nitride in this furnace, and the particles level is therefore low compared to the older nitride furnace
*Before running a process keep in close contact with the Danchip staff (especially the process specialist on the furnace) or take a look at the logbook to make sure that the nitride furnace is expected to be in a good state.


TEOS oxide has an amorphous crystal structure. If TEOS oxide is annealed at a high temperature, ~1000 <sup>o</sup>C, carbon is removed, and the crystal structure becomes more dense, and thus the thickness decreases. The quality of an annealed TEOS oxide film is actually almost similar to the quality of a thermal oxide film.


'''To avoid too rough handling of the wafers after the nitride deposition'''<br\>
There is one standard process for deposition of LPCVD TEOS oxide on the furnace, and this recipe is called "TEOS". The Thin Film group will have to be involved, if depositions have to done with other process parameters. The exact TEOS flow is unfortunately not know, but it is expected to be much higher than the setpoint in the recipe, because the MFC is not calibrated for TEOS (it has not been possible to buy a correctly calibrated MFC).
*After the deposition handle the wafers with a clean glove on the edge of the wafers (no tweezers).
*Be careful not to scratch wafers with nitride (e.g. up against each other or on the spinner or the aligner).
*If you have nitride on the back side of a wafer while aligning, consider if you can protect it with e.g. a photoresist layer before loading it onto the aligner. Or use a non-vacuum aligner chuck with a big hole in the middle, so that the wafer is only laying on the edge. Avoid hard contact in the aligner if possible.


On the furnace there are also two standby recipes, which are used for wafer loading and unloading. One standby recipe is called "STANDBY". The other standby recipe is called "STB-SLOW", and this is being used, if a thicker TEOS oxide layer (> 1 µm) is deposited, because the furnace then has to open slower to avoid stress and thus cracks in the deposited film.


'''To avoid too much stress between the nitride and the underlying layer'''<br\>
==Process parameters standard deposition recipes and the standby recipes on the TEOS furnace:==
*It is recommended to have a of silicon oxide layer between the silicon substrate and the nitride layer to reduce the stress level between the layers. The silicon nitride is then expected to have less tendency to break.


{| border="1" cellspacing="0" cellpadding="4"
!Recipe name
!Wafer size and number of wafers
!Temperature [<sup>o</sup>C]
!Pressure [mTorr]
!TEOS gas flow [sccm]
!O<sub>2</sub> gas flow [sccm]
!Comments
|-
| "STANDBY" and "STB-SLOW"
(standby recipes)
| 4" wafers
1-15 wafers
| 560 <sup>o</sup>C
(wafer loading temperature)
| Atmospheric pressure
(wafer loading pressure)
| 0 sccm
| 0 sccm
| For wafer loading and unloading
|-
| "TEOS"
(deposition recipe)
| 4" wafers
1-15 wafers
| 715, 712, 720 <sup>o</sup>C
(temperature zone 1, 2, 3)
| 175 mTorr
| 50 sccm. <i>The exact flow is not know - the setpoint is much lower than 50 sccm, but the MFC is not calibrated for TEOS</i>
| 0 sccm
| Process recipe
|}


==Deposition rate and refractive index:==


The deposition rate is normally a little below 10 nm/min - See process log in LabManager. But especially for short depositions, the deposition rate is higher and depends on the deposition time. The main reason for this is that there is some TEOS (about 20-30 nm) being deposited during the pre- and post-deposition steps in the recipe, and this does not count as deposition time. The post-deposition step is when the TEOS is introduced into the furnace tube before the deposition, and the pre-deposition step is when the TEOS gas line and MFC are emptied through the furnace tube after the deposition.


Before you use the furnace, it is recommended to look at process log to find the latest deposition rates.


for sjov
The refractive index is around 1.44.
 
<math>
\mathcal{V}^\prime=-\sqrt{rcs}A\cosh(\sqrt{rcs}(L-x))-\sqrt{rcs}B\sinh(\sqrt{rcs}(L-x))
</math>
 
 
<math> Z=\frac{\mathcal{V}(0)}{\mathcal{I}(0)}=rL\frac{B\cosh(\sqrt{rcs}L)}{\sqrt{rcs}LB\sinh(\sqrt{rcs}L)} </math>
 
[[image:RIE1_Si_Angle_O2_CHF3.jpg|300x300px|thumb|right|Angle of sidewall on 1.5 µm trenches - independent on pressure within the given pressure range]]
 


<math>
TEOS has compressive stress (around 100-300 MPa).


\includegraphics[width=0.5\textwidth]{RIE1_Si_Angle_O2_CHF3.jpg}
==Using LPCVD TEOS oxide as a masking material for KOH etching==
\caption{The simplified model, which can be used in stead of the
one in figure. In this representation is
the total resistance in the entire transmission lines, not just
between the capacitors.}


</math>
It is possible to use LPCVD TEOS oxide as a masking layer for KOH etching. However, it is not as suitable as LPCVD silicon nitride for deep KOH etching, as the etch rate for TEOS oxide is higher than the etch rate for silicon nitride.

Latest revision as of 15:58, 10 January 2025

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal

LPCVD TEOS oxide deposition

Figure 1: TEOS molecule structure
Figure 2: LPCVD TEOS oxide deposited on Si trenches

DTU Nanolab has one furnace for deposition of LPCVD TEOS oxide. The furnace is a Tempress horizontal furnace, and it was installed in the cleanroom in 1995.

In the furnace LPCVD TEOS oxide can be deposited on up to 15 4" wafers. It is not possible to deposit TEOS oxide on 6" wafers in he cleanroom.

TEOS is is Tetra-Ethyl-Ortho-Silicate, sometimes also referred to as Tetra-Ethoxy-Silane, and it has the chemical formula Si(C2H5O)4. The molecular structure can be seen figure 1. It is a liquid that is stored in a bubbler. When a deposition is started, the bubbler is heated to 75 oC, and TEOS is then vaporized and introduced into the furnace. The TEOS flow is controlled by an MFC (mass flow controller).

In the furnace, TEOS is thermally decomposed on the sample surface, so that a layer of silicon dioxide (SiO2) is deposited there:

Si(C2H5O)4 (l) → SiO2 (s) + 4 CH2H4 (g) + 2 H2O (g)

Carbon can be incorporated in the TEOS oxide layer, but this can be reduced by an annealing - see below.

The difference between TEOS and silane gas (used for deposition of silicon nitride) is essentially that in TEOS the silicon atom is already oxidized. Therefore the conversion of TEOS to silicon dioxide is a rearrangement rather than an oxidation. As can be seen from figure 1 what is basically required to deposit silicon dioxide is a removal of two oxygen atoms, and for that to happen a relative high temperature of 720 oC is needed.

TEOS molecules have a very high surface mobility enabling the TEOS oxide to fill holes that have a large aspect ratio and leaving the surface quite smooth, see figure 2, hence it also covers corners and side walls very well. However very small nanometer trenched and/or very deep trenches will be challenging to fill.

TEOS oxide has an amorphous crystal structure. If TEOS oxide is annealed at a high temperature, ~1000 oC, carbon is removed, and the crystal structure becomes more dense, and thus the thickness decreases. The quality of an annealed TEOS oxide film is actually almost similar to the quality of a thermal oxide film.

There is one standard process for deposition of LPCVD TEOS oxide on the furnace, and this recipe is called "TEOS". The Thin Film group will have to be involved, if depositions have to done with other process parameters. The exact TEOS flow is unfortunately not know, but it is expected to be much higher than the setpoint in the recipe, because the MFC is not calibrated for TEOS (it has not been possible to buy a correctly calibrated MFC).

On the furnace there are also two standby recipes, which are used for wafer loading and unloading. One standby recipe is called "STANDBY". The other standby recipe is called "STB-SLOW", and this is being used, if a thicker TEOS oxide layer (> 1 µm) is deposited, because the furnace then has to open slower to avoid stress and thus cracks in the deposited film.

Process parameters standard deposition recipes and the standby recipes on the TEOS furnace:

Recipe name Wafer size and number of wafers Temperature [oC] Pressure [mTorr] TEOS gas flow [sccm] O2 gas flow [sccm] Comments
"STANDBY" and "STB-SLOW"

(standby recipes)

4" wafers

1-15 wafers

560 oC

(wafer loading temperature)

Atmospheric pressure

(wafer loading pressure)

0 sccm 0 sccm For wafer loading and unloading
"TEOS"

(deposition recipe)

4" wafers

1-15 wafers

715, 712, 720 oC

(temperature zone 1, 2, 3)

175 mTorr 50 sccm. The exact flow is not know - the setpoint is much lower than 50 sccm, but the MFC is not calibrated for TEOS 0 sccm Process recipe

Deposition rate and refractive index:

The deposition rate is normally a little below 10 nm/min - See process log in LabManager. But especially for short depositions, the deposition rate is higher and depends on the deposition time. The main reason for this is that there is some TEOS (about 20-30 nm) being deposited during the pre- and post-deposition steps in the recipe, and this does not count as deposition time. The post-deposition step is when the TEOS is introduced into the furnace tube before the deposition, and the pre-deposition step is when the TEOS gas line and MFC are emptied through the furnace tube after the deposition.

Before you use the furnace, it is recommended to look at process log to find the latest deposition rates.

The refractive index is around 1.44.

TEOS has compressive stress (around 100-300 MPa).

Using LPCVD TEOS oxide as a masking material for KOH etching

It is possible to use LPCVD TEOS oxide as a masking layer for KOH etching. However, it is not as suitable as LPCVD silicon nitride for deep KOH etching, as the etch rate for TEOS oxide is higher than the etch rate for silicon nitride.