Jump to content

Specific Process Knowledge/Thin film deposition/Furnace LPCVD PolySilicon/Boron doped poly-Si and a-Si: Difference between revisions

From LabAdviser
Paphol (talk | contribs)
No edit summary
Mmat (talk | contribs)
mNo edit summary
 
(16 intermediate revisions by 3 users not shown)
Line 1: Line 1:
{{cc-nanolab}}
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_PolySilicon/Boron_doped_poly-Si_and_a-Si click here]'''


==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
==Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
''Result from Thomas Pedersen, @Nanotech, Sep 2015''
''Result from Thomas Pedersen, DTU Nanotech (now DTU Nanolab), September 2015''
====Process parameters====
====Process parameters====


Line 30: Line 33:


[[image:Boron concentration2.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.]]
[[image:Boron concentration2.jpg|627x424px|left|thumb|Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.]]
<br clear="all" />
== Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4) ==
''Result from Trine Holm Christensen, @Space, Feb. 2015''
====Process parameters====
The test was made on a n-type silicon wafer (100) with a 110 nm grown thermal oxide)
'''Pressure:'''  250 mtorr
'''Temperature:''' 580 °C
'''Silane (SiH<sub>4</sub>) flow:''' 80 sccm
'''Diborane (B<sub>2</sub>H<sub>6</sub>) flow:''' 7 sccm
'''Time:''' 75 min
'''Anneal:''' @950°C for 60 min in N<sub>2</sub>
'''Test wafer position:''' Center of the boat
A better uniformity of the resistivity across the wafer was achieved by subsequently annealing in N<sub>2</sub>, the annealing was done in Anneal Oxide Furnace (C1). The measured film thickness was 370 nm and the sheet resistance was measured to 200 &Omega;/sq +/- 15 &Omega;/sq.

Latest revision as of 14:24, 6 March 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here


Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4)

Result from Thomas Pedersen, DTU Nanotech (now DTU Nanolab), September 2015

Process parameters

Pressure: 250 mtorr

Temperature: 580 °C

Silane (SiH4) flow: Constant at 80 sccm

Diborane (B2H6) flow: Varied from 3 sccm to 40 sccm

Anneal: No annealing afterwards

Test wafer position: Center of the boat

Results

The Boron concentration of the film was controlled by the flow of B2H6 gas. To establish how boron doping concentration varied with B2H6 flow, films of silicon were deposited with B2H6 gas flows modulated during deposition to produce doping spikes. The two figures below show a typical SIMS concentration depth profile of a B2H6 modulation-doped film deposited on a Silicon dioxide substrate. During deposition, the gas flow of SiH4 was held constant, while flows of B2H6 was varied to create the dopant spikes.


Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.


Boron concentration measured by SIMS. Result from Thomas Pedersen, Nanotech, Sep 2015.


Boron-doped amorphous silicon by using 4" LPCVD polysilicon furnace (B4)

Result from Trine Holm Christensen, @Space, Feb. 2015

Process parameters

The test was made on a n-type silicon wafer (100) with a 110 nm grown thermal oxide)

Pressure: 250 mtorr

Temperature: 580 °C

Silane (SiH4) flow: 80 sccm

Diborane (B2H6) flow: 7 sccm

Time: 75 min

Anneal: @950°C for 60 min in N2

Test wafer position: Center of the boat

A better uniformity of the resistivity across the wafer was achieved by subsequently annealing in N2, the annealing was done in Anneal Oxide Furnace (C1). The measured film thickness was 370 nm and the sheet resistance was measured to 200 Ω/sq +/- 15 Ω/sq.