Specific Process Knowledge/Thin film deposition/ALD Picosun R200/Standard recipes on the ALD tool: Difference between revisions
Line 396: | Line 396: | ||
=ZnO (Zinc oxide)= | =ZnO (Zinc oxide)= | ||
==ZnO deposition using DEZ | ==Standard ZnO deposition using DEZ and H<sub>2</sub>O precursors== | ||
Line 427: | Line 427: | ||
This is a standard recipe of ZnO. It is suitable for coating the flat samples and structures with an aspect ratio of around up to 1:10. | This is a standard recipe of ZnO. It is suitable for coating the flat samples and structures with an aspect ratio of around up to 1:10. | ||
==ZnO deposition on high aspect ratio structures using DEZ and H<sub>2</sub>O precursors= | |||
<b>Recipe name: ZnOT</b> | <b>Recipe name: ZnOT</b> |
Revision as of 12:24, 4 March 2022
Feedback to this page: click here
Al2O3 (Aluminium oxide)
Al2O3 deposition using TMA and H2O precursors
Recipe name: AL2O3
Temperature window: 150 oC - 350 oC
TMA | H2O | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s |
Purge time | 3.0 s | 4.0 s |
Al2O3 deposition using TMA and O3 precursors
Recipe name: AL2O3O3
Temperature window: 300 oC - 350 oC
TMA | O3 | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.2 s | 0.1 s |
Purge time | 3.0 s | 4.0 s |
Al2O3 deposition on high aspect ratio structures using TMA and H2O precursors
Recipe name: AL2O3T
Temperature window: 150 oC - 350 oC
TMA | TMA | H2O | H2O | |
---|---|---|---|---|
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
TiO2 (Titanium dioxide)
TiO2 deposition using TiCl4 and H2O precursors
Recipe name: TIO2
Temperature window: 120 oC - 150 oC (amorphous TiO2), 300 oC - 350 oC (anatase TiO2)
TiCl4 | H2O | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s |
Purge time | 4.0 s | 5.0 s |
TiO2 deposition on high aspect ratio structures using TiCl4 H2O precursors
Recipe name: TIO2T
Temperature window: 120 oC -150 oC (amorphous TiO2), 300 oC - 350 oC (anatase TiO2)
TiCl4 | TiCl4 | H2O | H2O | |
---|---|---|---|---|
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
HfO2 (Hafnium oxide)
HfO2 deposition using TEMAHf and H2O precursors
Recipe names: HFO2-150, HFO2-200, HFO2-250, HFO-300, HFO-350
Temperature window: 150 oC - 350 oC
Recipe for deposition of HfO2 at 150 oC | ||||||||||||||||||||||||||||||||||||||
|
Recipe for deposition of HfO2 at 200 oC | ||||||||||||||||||||||||||||||||||||||
|
Recipe for deposition of HfO2 at 250 oC - 350 oC | ||||||||||||||||||||||||||||||||||||||
|
The TEMAHf precursor is heated to 125 oC (TE210) and the heater (TE211 max.) is set to 150 oC during deposition. Remember to set the values in the "MANUAL" tab and to change them to back after deposition (TE211 max. to 1 oC). These values may not be exceeded to prevent precursor decomposition. Due to the heating of the precursor, the stabilization time needs to be set to at least 60 min. Else an alarm (TE210 PID limit exceeded while pulsing) will be triggered and the process will be stopped after the first pulsing attempt.
Further information can be found here:
HfO2 deposition using TEMAHf and H2O precursors
ZnO (Zinc oxide)
Standard ZnO deposition using DEZ and H2O precursors
Recipe name: ZnO
Maximum deposition thickness: 100 nm
Temperature: 100 oC - 250 oC
DEZ* | H2O | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s |
Purge time | 5.0 s | 5.0 s |
This is a standard recipe of ZnO. It is suitable for coating the flat samples and structures with an aspect ratio of around up to 1:10.
=ZnO deposition on high aspect ratio structures using DEZ and H2O precursors
Recipe name: ZnOT
Maximum deposition thickness: 100 nm
Temperature: 100 oC - 250 oC
DEZ* | DEZ | H2O | H2O | |
---|---|---|---|---|
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
This is a more complicated recipe that allows coating the sample with very high aspect ratio profiles. One SEM example is shown on one of the images below. The recipe is good for deposition on very high aspect ratio structures (with aspect ratio more than 1:20) such as deep trenches, pillars, pores etc. ZnOT recipe can also be used for deposition on polymers at low temperatures (80-120 oC).
DEZ is diethylzinc Zn(CH2CH3)2 or ZnEt2
Al-doped ZnO (AZO)
Al-doped ZnO deposition using DEZ, TMA and H2O precursors
Recipe: AZO 20T
(Number 20 means doping level "D": 19 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Temperature window: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 19 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 19 = 3.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 19] + [(0.1 + 0.1) s * 1] = 4.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 25T
Number 25 means doping level "D": 14 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Temperature: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 24 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 24 = 4.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 24] + [(0.1 + 0.1) s * 1] = 5.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 30T
(Number 30 means doping level "D": 29 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Temperature: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 29 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 29 = 5.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 29] + [(0.1 + 0.1) s * 1] = 6.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).
Recipe: AZO 35T
(Number 35 means doping level "D": 34 cycles of ZnO + 1 cycle Al2O3, see details in the table below)
Temperature: 150 oC - 250 oC
# macrocycles | N | |||||||
---|---|---|---|---|---|---|---|---|
# cycles | 34 | 1 | ||||||
Precursor | DEZ | DEZ | H2O | H2O | TMA | TMA | H2O | H2O |
Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Purge time | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s | 0.5 s | 20.0 s |
How to fill out the process log in LabManager:
The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.
DEZ pulse time: (0.1 + 0.1) s * 34 = 6.8 s
TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s
H2O pulse time: [(0.1 + 0.1) s * 34] + [(0.1 + 0.1) s * 1] = 7.0 s
The number of cycles for each precursor now equals the number of macrocycles (n).