Specific Process Knowledge/Lithography/Espacer: Difference between revisions
No edit summary |
No edit summary |
||
Line 41: | Line 41: | ||
|-style="background:WhiteSmoke; text-align:center; color:black" | |-style="background:WhiteSmoke; text-align:center; color:black" | ||
|E-beam exposure | |E-beam exposure | ||
|colspan="2"|2 nA, aperture 5, dose 150-310 muC/cm2, SHOT A,10 | |colspan="2"|2 nA, aperture 5, dose 150-310 muC/cm2, SHOT (A,10) | ||
|- | |- | ||
Revision as of 08:36, 11 July 2014
We have Espacer in stock and approved for use in the cleanroom. You can find a guideline for a process flow here: Process_Flow_ZEP_ESPACER.docx. Technical information of Espacer can be found here: Espacer_300_Technical_Info.pdf, Espacer_catalog.pdf.
Please contact Lithography if you wish to test this material.
Process | No ESPACER | ESPACER |
---|---|---|
Resist | Borofloat 4" wafers (JB456), no pretreatment | |
Resist | AR-P 6200/2 AllResist E-beam resist | |
Spin Coat | 1 min @ 4000 rpm, softbake 2 min @ 150 degC, thickness ~140nm | |
ESPACER | 1 min @ 2000 rpm (no softbake), Manual Spinner 1 (Laurell) | |
E-beam exposure | 2 nA, aperture 5, dose 150-310 muC/cm2, SHOT (A,10) | |
Rinse | Rinsed with hand shower in fumehood, dried with N2 gun | |
Developing | SX-AR 600-54/6 60 sec, 60 sec IPA rinse | |
Characterization | Nikon ECLIPSE optical microscope, E-5 | |
All doses | ||
230 muC/cm2 | ||
219 muC/cm2 | ||
Sputter Coated | <10nm Pt at DTU CEN | |
Characterization | Zeiss SEM supra 60VP, D-2 | |
230 muC/cm2 |