Specific Process Knowledge/Lithography/Espacer: Difference between revisions

From LabAdviser
Tigre (talk | contribs)
No edit summary
Tigre (talk | contribs)
No edit summary
Line 41: Line 41:
|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|E-beam exposure
|E-beam exposure
|colspan="2"|2 nA, aperture 5, dose 150-310 muC/cm2, SHOT A,10
|colspan="2"|2 nA, aperture 5, dose 150-310 muC/cm2, SHOT (A,10)
|-
|-



Revision as of 08:36, 11 July 2014

We have Espacer in stock and approved for use in the cleanroom. You can find a guideline for a process flow here: Process_Flow_ZEP_ESPACER.docx‎. Technical information of Espacer can be found here: Espacer_300_Technical_Info.pdf‎, Espacer_catalog.pdf‎.

Please contact Lithography if you wish to test this material.


Process No ESPACER ESPACER
Resist Borofloat 4" wafers (JB456), no pretreatment
Resist AR-P 6200/2 AllResist E-beam resist
Spin Coat 1 min @ 4000 rpm, softbake 2 min @ 150 degC, thickness ~140nm
ESPACER 1 min @ 2000 rpm (no softbake), Manual Spinner 1 (Laurell)
E-beam exposure 2 nA, aperture 5, dose 150-310 muC/cm2, SHOT (A,10)
Rinse Rinsed with hand shower in fumehood, dried with N2 gun
Developing SX-AR 600-54/6 60 sec, 60 sec IPA rinse
Characterization Nikon ECLIPSE optical microscope, E-5
All doses
230 muC/cm2
219 muC/cm2
Sputter Coated <10nm Pt at DTU CEN
Characterization Zeiss SEM supra 60VP, D-2
230 muC/cm2