|ESPACER
|
|
|1 min @ 2000 rpm (no softbake)
|1 min @ 2000 rpm (no softbake), [[Specific Process Knowledge/Lithography/Coaters#Manual Spinner 1 (Laurell)|Manual Spinner 1 (Laurell)]]
|-
|-



Revision as of 09:22, 10 July 2014

We have ESPACER in stock and approved for use in the cleanroom. You can find a guideline for a process flow here: Process_Flow_ZEP_ESPACER.docx‎. Technical information of EPSCAER can be found here: Espacer_300_Technical_Info.pdf‎, Espacer_catalog.pdf‎.

Please contact Lithography if you wish to test this material.


Process No ESPACER ESPACER
Resist AR-P 6200/2 AllResist E-beam resist
Spin Coat 1 min @ 4000 rpm, softbake 2 min @ 150 degC, thickness ~140nm
ESPACER 1 min @ 2000 rpm (no softbake), Manual Spinner 1 (Laurell)
E-beam exposure 2 nA, aperture 5, dose 150-310 muC/cm2, SHOT A,10
Rinse Rinsed with hand shower in fumehood, dried with N2 gun
Developing SX-AR 600-54/6 60 sec, 60 sec IPA rinse
Characterization Nikon ECLIPSE optical microscope, E-5