Specific Process Knowledge/Thin film deposition/Deposition of Titanium Oxide: Difference between revisions
No edit summary |
|||
(5 intermediate revisions by the same user not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Titanium_Oxide click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Titanium_Oxide click here]''' | ||
''All contents by '''Nanolab staff | ''All contents by '''Nanolab staff.''''' | ||
==Deposition of Titanium Oxide== | ==Deposition of Titanium Oxide== | ||
Titanium oxide can be deposited | Titanium oxide can be deposited at Nanolab by sputtering, e-beam deposition, or ALD (atomic layer deposition). In sputtering and e-beam deposition of titanium oxide, the target is Ti and oxygen is added to the chamber during the process resulting in Titanium oxide on the sample. Therefore some process development may be necessary to achieve the correct stoichiometry. The oxygen flow in e-beam evaporation is lower than in sputtering, so it may not be possible to obtain fully oxidized TiO<sub>2</sub>, though we have not yet verified this. | ||
*[[Specific Process Knowledge/Thin film deposition/ALD Picosun R200/TiO2 deposition using ALD|TiO2 deposition using ALD]] | *[[Specific Process Knowledge/Thin film deposition/ALD Picosun R200/TiO2 deposition using ALD|TiO2 deposition using ALD]] | ||
*[[Specific Process Knowledge/Thin film deposition/TiO2 deposition using Sputter-System Metal-Oxide(PC1)|TiO2 deposition using Sputter-System Metal-Oxide(PC1)]] | *[[Specific Process Knowledge/Thin film deposition/TiO2 deposition using Sputter-System Metal-Oxide(PC1)|TiO2 deposition using Sputter-System Metal-Oxide(PC1)]] | ||
*[[Specific Process Knowledge/Thin film deposition/TiO2 deposition in Sputter System (Lesker)|TiO2 deposition in Sputter System (Lesker)]] | *[[Specific Process Knowledge/Thin film deposition/TiO2 deposition in Sputter System (Lesker)|TiO2 deposition in Sputter System (Lesker)]] | ||
We also used to have the option to sputter-deposit [[/IBSD of TiO2|TiO2 with the IBE/IBSD Ionfab300]]. | |||
==Comparison of the methods for deposition of Titanium Oxide== | ==Comparison of the methods for deposition of Titanium Oxide== | ||
Line 18: | Line 19: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
! | ![[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]] | ||
![[Specific Process Knowledge/Thin film deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-system Metal-Oxide(PC1)]] | ![[Specific Process Knowledge/Thin film deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system|Sputter-system Metal-Oxide(PC1)]] | ||
![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] | ![[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System(Lesker)]] | ||
Line 28: | Line 29: | ||
!Generel description | !Generel description | ||
| | | | ||
*TiO<sub>2</sub> | *Evaporation of Ti or TiO<sub>2</sub> pellets in the presence of a O<sub>2</sub> flow. | ||
| | | | ||
*Reactive DC sputtering of Ti target | *Reactive DC sputtering of Ti target | ||
*Reactive or non-reactive RF sputtering of | *Reactive or non-reactive RF sputtering of TiO<sub>2</sub> target | ||
*Reactive pulsed DC sputtering | *Reactive pulsed DC sputtering | ||
*Reactive HIPIMS (high-power impulse magnetron sputtering) | *Reactive HIPIMS (high-power impulse magnetron sputtering) | ||
| | | | ||
*Reactive DC sputtering of Ti target in Ar/ | *Reactive DC sputtering of Ti target in Ar/O<sub>2</sub> (10 % O<sub>2</sub>) plasma | ||
*RF sputtering of | *RF sputtering of TiO<sub>2</sub> target | ||
| | | | ||
*ALD (atomic layer deposition) of TiO<sub>2</sub> | *ALD (atomic layer deposition) of TiO<sub>2</sub> | ||
Line 45: | Line 46: | ||
!Stoichiometry | !Stoichiometry | ||
| | | | ||
*Can probably be varied | *Can probably be varied, expect somewhat O-poor composition | ||
| | | | ||
*Can probably be varied | *Can probably be varied | ||
Line 58: | Line 59: | ||
!Film Thickness | !Film Thickness | ||
| | | | ||
* | *few nm - 100 nm | ||
| | | | ||
*~10 nm - ~0.5 µm | *~10 nm - ~0.5 µm | ||
Line 64: | Line 65: | ||
*~10 nm - ~0.5 µm (>2h) | *~10 nm - ~0.5 µm (>2h) | ||
| | | | ||
* | * few nm - 100 nm | ||
|- | |- | ||
Line 70: | Line 71: | ||
!Deposition rate | !Deposition rate | ||
| | | | ||
* | *1-10 Å/s Ti deposition rate (oxidized layer growth should be faster; actual growth rate will need testing) | ||
| | | | ||
*not yet known, probably faster than Sputter-System(Lesker) | *not yet known, probably faster than Sputter-System(Lesker) | ||
Line 84: | Line 85: | ||
!Step coverage | !Step coverage | ||
| | | | ||
* | *expect no step coverage unless the tilted sample holder is used, in which case step coverage should be very good and may be tuned with the tilt angle. | ||
| | | | ||
*Not Known | *Not Known | ||
Line 96: | Line 97: | ||
!Process Temperature | !Process Temperature | ||
| | | | ||
* | *RT to 250 °C | ||
| | | | ||
*RT to 600 °C | *RT to 600 °C | ||
| | | | ||
*RT | *RT | ||
| | | | ||
*120 °C - 150 °C: Amorphous TiO<sub>2</sub> | *120 °C - 150 °C: Amorphous TiO<sub>2</sub> | ||
Line 110: | Line 111: | ||
!More info on TiO2 | !More info on TiO2 | ||
| | | | ||
* | *Expect lower density than bulk material of same stoichiometry. | ||
| | | | ||
*[[Specific Process Knowledge/Thin film deposition/TiO2 deposition using Sputter-System Metal-Oxide(PC1)|TiO2 deposition using Sputter-System Metal-Oxide(PC1)]] | *[[Specific Process Knowledge/Thin film deposition/TiO2 deposition using Sputter-System Metal-Oxide(PC1)|TiO2 deposition using Sputter-System Metal-Oxide(PC1)]] | ||
Line 126: | Line 127: | ||
!Substrate size | !Substrate size | ||
| | | | ||
* | *Up to 4x6" wafers | ||
* | *Up to 3x8" wafers (ask for holder) | ||
* | *smaller pieces | ||
| | | | ||
*many small samples | *many small samples | ||
Line 157: | Line 156: | ||
!Allowed materials | !Allowed materials | ||
| | | | ||
*Almost any | *Almost any material that does not outgas at your intended substrate temperature and is not toxic | ||
* | *See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet] | ||
| | | | ||
*Almost any | *Almost any material that does not outgas at your intended substrate temperature | ||
*Pb and | *Pb and other toxic materials only after special agreement | ||
| | | | ||
*Almost any that do not outgas and are not very | *Almost any that do not outgas and are not very toxic | ||
*Dedicated carrier for III-V materials | *Dedicated carrier for III-V materials | ||
*See [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 cross-contamination sheet] | *See [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 cross-contamination sheet] |
Revision as of 13:11, 4 July 2024
Feedback to this page: click here
All contents by Nanolab staff.
Deposition of Titanium Oxide
Titanium oxide can be deposited at Nanolab by sputtering, e-beam deposition, or ALD (atomic layer deposition). In sputtering and e-beam deposition of titanium oxide, the target is Ti and oxygen is added to the chamber during the process resulting in Titanium oxide on the sample. Therefore some process development may be necessary to achieve the correct stoichiometry. The oxygen flow in e-beam evaporation is lower than in sputtering, so it may not be possible to obtain fully oxidized TiO2, though we have not yet verified this.
- TiO2 deposition using ALD
- TiO2 deposition using Sputter-System Metal-Oxide(PC1)
- TiO2 deposition in Sputter System (Lesker)
We also used to have the option to sputter-deposit TiO2 with the IBE/IBSD Ionfab300.
Comparison of the methods for deposition of Titanium Oxide
E-beam evaporator (10-pockets) | Sputter-system Metal-Oxide(PC1) | Sputter-System(Lesker) | ALD Picosun 200 | |
---|---|---|---|---|
Generel description |
|
|
|
|
Stoichiometry |
|
|
|
|
Film Thickness |
|
|
|
|
Deposition rate |
|
|
|
|
Step coverage |
|
|
|
|
Process Temperature |
|
|
|
|
More info on TiO2 |
|
|
ALD1: ALD2: | |
Substrate size |
|
|
|
ALD1:
ALD2:
|
Allowed materials |
|
|
|
|