The furnace A4 phosphorus predep(N-predep) can be used to predeposit silicon wafers with phosphor. The silicon wafers are positioned in a quarts boat. Phosphor is predeposited in the silicon wafers.
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thermal_Process/Dope_with_Phosphorus click here]'''


'''
== In preparation ==
'''
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=


<!--
The Phosphorus Predep furnace (A4) can be used for phosphorus pre-deposition of silicon wafers, resulting in n-type doping. In the furnace, the silicon wafers are positioned vertically in a quarts boat.
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Bge-Under construction.jpg|200px]]=
 
-->


'''
'''
==Test of Phosphorus Predep furnace==
==Test of the Phosphorus Predep furnace==
'''
'''
'''
'''
''This page is written by DTU Nanolab  internal''
====Purpose====
====Purpose====
'''  
'''  


To study the coherence between the temperature of the Predep and dive-in for doping with phosphorus in DTU-Danchip Phosphorus Predep furnace (A4).  
To study the correlation between the temperature for the predeposition process and drive-in of the phosphorus doping in the Phosphorus Predep furnace (A4) at DTU Nanolab.  


'''
'''


====Experiment setup====
====Experimental setup====
'''
'''
There was used 20 boron doped wafers (p-type). There was used four wafer to the five different temperature. There was five dummy wafers on each side of the test wafers. The dummy wafer nearest to the test wafers was changed in between the runes so doping from a dummy wafer was minimized.  
20 boron doped device wafers (p-type) were used - Four wafers for each of the five different predeposition temperatures (see table below). In the furnace five dummy wafers were placed on each side of the device wafers. The dummy wafers nearest to the device wafers were changed in-between the runs to minimize doping from these dummy wafers.  


{| border="1" cellspacing="1" cellpadding="2" ||3||4||5
{| border="1" cellspacing="1" cellpadding="2" style="text-align:center;" width="690" ||3||4||5
|Run #||Temperature||Process time with POCl3||Anneal time N2||Wafer #
!| Run #||Temperature||Process time with POCl<sub>3</sub>||Annealing time in O<sub>2</sub>||Wafer #
|-
|-  
|1||850 <sup>o</sup>C||15 minutes||20 miuntes||1, 2, 3, 4
|1||850 <sup>o</sup>C||15 minutes||20 minutes||1, 2, 3, 4
|-  
|-  
|2||900 <sup>o</sup>C||15 minutes||20 miuntes||5, 6, 7, 8  
|2||900 <sup>o</sup>C||15 minutes||20 minutes||5, 6, 7, 8  
|-
|-
|3||950 <sup>o</sup>C||15 minutes||20 miuntes||9, 10, 11, 12  
|3||950 <sup>o</sup>C||15 minutes||20 minutes||9, 10, 11, 12  
|-
|-
|4||1000 <sup>o</sup>C||15 minutes||20 miuntes||13, 14, 15, 16
|4||1000 <sup>o</sup>C||15 minutes||20 minuntes||13, 14, 15, 16
|-
|-
|5||1050 <sup>o</sup>C||15 minutes||20 miuntes||17, 18, 19, 20
|5||1050 <sup>o</sup>C||15 minutes||20 minutes||17, 18, 19, 20
|}
|}
'''
'''
After the Predep was two wafer from each run taken out to be further processed. The wafers was 1, 2, 5, 6, 9, 10, 13, 14, 17, 18.  
After the predeposition two wafers from each run were taken out to be further processed. These wafers were: 1, 2, 5, 6, 9, 10, 13, 14, 17, 18. These wafers were dipped in BHF to remove the phosphorus glass layer before the drive-in process.  


These wafers was dipped in BHF to get the phosphorus glass layer of before the Drive-in process. The Drive-in process was made in Danchip Phosphorus Drive-in furnace (A3). There was a dummy wafer in between the wafers from different temperatures so doping from wafer to wafer was minimized. The Drive-in was done with the process "DRY1050" with is a dry oxidation at 1050 <sup>o</sup>C for 100 minutes and 20 minutes annealing. At the oxdation was the O<sub>2</sub> flow was 5 SLM and N<sub>2</sub> flow for annealing was 3 SLM.
The drive-in process was made in the Phosphorus Drive-in furnace (A3) for all the mentioned wafers at same time. At the drive-in process a dummy wafer was placed in-between the wafers that have been predeposited at different temperatures, so doping from wafer to wafer was minimized. The phosphorus drive-in was done with the process "DRY1050" which is a dry oxidation at 1050 <sup>o</sup>C for 100 minutes and 20 minutes annealing. At the oxidation the O<sub>2</sub> flow was 5 SLM, and the N<sub>2</sub> flow for annealing was 3 SLM.


====Test measurement====
====Results====
'''
'''
There was made several measurement on the different wafer in the process. After the predep was the oxide thickness, sheet resistance and slice resistivity measured on some of the wafer.  
Several measurements were done for the different device wafers. After the predeposition, the thickness of the grown phosphorus glass layer was measured, and the sheet resistance and slice resistivity were measured on the same wafer after a BHF etch.  
 


{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|+ '''Measurement after Predep'''
|+ '''Measurements after phosphorus predeposition'''
|-
|-
!  
!  
! colspan="2" | Elipsometer
!
! colspan="2" | Ellipsometer (center point only)
! colspan="2" | Four Point Probe  
! colspan="2" | Four Point Probe  
|-
|-
! width="120" | Wafer #
! width="130" | Wafer #  
! width="120" | Thinkness [nm]
! width="130" | Temperature [C]
! width="120" | Refrative index
! width="130" | Oxide thickness [nm]
! width="120" | Sheet  
! width="130" | Refractive index
! width="120" | Slice
! width="150" | Sheet resistance [&Omega;<sub>sq</sub>]
! width="150" | Slice Resistivity [&Omega;cm]
|-
|-
! 3  
! 3  
| 850
| 27,4  
| 27,4  
| 1,4623
| 1,4623
| 311
| 311
| 17,32
| 6,22*10<sup>-3</sup>
|-
|-
! 7  
! 7  
| 900
| 45,27
| 45,27
| 1,4622
| 1,4622
| 138,5
| 138,5
| 7,61
| 4,85*10<sup>-3</sup>
|-
|-
! 11  
! 11  
| 950
| 61,36
| 61,36
| 1,4625
| 1,4625
| 16,12
| 16,1
| 0,859
| 1,29*10<sup>-3</sup>
|-
|-
! 15  
! 15  
| 1000
| 80,45
| 80,45
| 1,4624
| 1,4624
| 7,4
| 7,4
| 0,392
| 0,89*10<sup>-3</sup>
|-
|-
! 19
! 19
| 1050
| 119,37
| 119,37
| 1,4623
| 1,4623
| 6,6
| 6,6
| 0,246
| 1,49*10<sup>-3</sup>
|-
|}
 
The oxide layer was etch in BHF before the drive-in of the doping with a dry oxidation at 1050 <sup>o</sup>C for 100 minutes and 20 minutes annealing.
 
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|+ '''Measurements after phosphorus drive-in'''
|-
!
!
! colspan="2" | Avg. five point on Filmtek
! colspan="2" | Four Point Probe
|-
! width="130" | Wafer # 
! width="130" | Temperature [<sup>o</sup>C]
! width="130" | Oxide thickness [nm]
! width="130" | Refractive index
! width="150" | Sheet resistance [&Omega;<sub>sq</sub>]
! width="150" | Slice Resistivity [&Omega;cm]
|-
! 2
| 850
| 110,44
| 1,4654
| 189,7
| 3,79*10<sup>-3</sup>
|-
! 6
| 900
| 116,28
| 1,4629
| 101,6
| 3,56*10<sup>-3</sup>
|-
! 9
| 950
| 137,06
| 1,4604
| 10,0
| 0,8*10<sup>-3</sup>
|-
! 14
| 1000
| 141,46
| 1,4651
| 4,72
| 0,57*10<sup>-3</sup>
|-
! 18
| 1050
| 139,87
| 1,4659
| 3,23
| 0,73*10<sup>-3</sup>
|-
! Blank Si wafer
|
| 110,71
| 1,46286
| -
| -
|-
|}
 
'''
'''
'''
 
 
 
{| border="1" cellspacing="1" cellpadding="2"  align="left"
|-
|[[image:Resistivity.png|400x400px|right|thumb|Resistivity]]||[[image:Sheet_resistance.png|400x400px|right|thumb|Sheet resistance]]
|-
|[[image:SIMS Measurement_After_Pre-dep.png|400x400px|right|thumb|SIMS Measurement After Pre-dep]]||[[image:SIMS Measurement_After_Drive-in_Process_at_1050_C.png|400x400px|right|thumb|SIMS Measurement After Drive-in Process at 1050 <sup>o</sup>C]]
|-
|}
 
<br clear="all" />
 
Looking at the "SIMS Measurement After Drive-in Process at 1050 <sup>o</sup>C" graph, it can be seen that the two curves "Pre-dep at 950 <sup>o</sup>C" and "Pre-dep at 1000 <sup>o</sup>C" are crossing each other, but according to the theory they should not do that. Only one wafer has been measured so there is not that much statistical data to verify it with.
 
<br clear="all" />
 
==Test of the Phosphorus Predep furnace==
'''
''This page is written by DTU Nanolab  internal''
 
====Purpose====
'''
 
To find the result of a specific process using the Phosphorus Predep furnace (A4) followed by a drive in and oxidating the substrate in the Phosphorus drive in furnace (A3).
'''
====Experimental setup====
'''
 
'''Substrate:''' p-type Si(100,)
 
'''Resistivity:''' 1-20 &Omega;cm
 
'''Recipe:'''  POCL900
 
'''Temperature:''' 900 °C
 
'''Time:''' 15 min
 
'''Anneal:''' 20 min in N<sub>2</sub>
 
After removing the oxide in BHF the wafers were oxidized in Phosphor Drive in Furnace (A3) using DRY1050 at 1050°C for 70 min without further annealing in N<sub>2</sub>. Results are listed in the table below:
 
====Results====
 
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;"
|+ '''Measurements after phosphorus predeposition'''
|-
!
! colspan="1" | Afer predeposition
! colspan="2" | After Oxidation
|-
! width="130" | Test date
! width="130" | Sheet resistance [&Omega;/sq]
! width="130" | Oxide thickness [nm]
! width="130" | Sheet resistance [&Omega;/sq
 
|-
! Aug2012
| 47.0
| 93.1
| 41.8
 
|-
! Jan2013
| 50.5
| 91.3
| 55.6
|-
! Aug2013
| 58.0
| 91.8
| 41.8
|-
! Jan2014
| 54.1
| 93.3
| 33.8
|-
! Jan2015
| 50.8
| 94.2
| 39.4
 
|-
|-
|}
|}
One wafer from Jan2015 was analyzed with SIMS and the profile is shown on the graph below:
[[image:Phosphorus_doping2015.jpg|500x600px|left|thumb|SIMS Measurement After Predeposition, before and after oxidation respectively]]
<br clear="all" />
''Result from GreenBelt, @nanolab,Jan 2015''
<br clear="all" />
==Test of the Phosphorus Predep furnace==
'''
====Purpose====
'''
To find the doping profile after a specific process flow. The test was made by only performing the high-temperature process step after the pre-deposition step done in the Phosphorus Predep furnace (A4). The subsequently high temperature processes was done by using the Phosphorous drive in furnace (A3) and the Oxide Anneal Furnace (C3).
'''
====Experimental setup====
'''
'''Substrate:''' p-type Si(100,)
'''Resistivity:''' 1-20 &Omega;cm
'''The total thermal budget for the wafers:'''
'''Predeposition in Furnace (A4):''' POCL1000, 15 min, no further anneal
'''Wet Oxidation in Furnace (A3)''': WET1050, 30 min, no further anneal
'''Anneal in Furnace (C1):''' ANN1000, 30 min in N<sub>2</sub>
'''Wet oxidation in Furnace (C1):''' WET1050, 30 min, no further anneal
====Results====
The wafer was analyzed with SIMS and the profile is shown on the graph below:
[[image:Phosphorous_doping_profile.jpg|500x600px|left|thumb|SIMS Measurement after Phosphorous Predeposition and several oxidations and annealings]]
<br clear="all" />
''Result from Trine Holm Christensen, @Space, Feb. 2015''
<br clear="all" />
==Phosphorous doping test after hardware and software upgrades==
''This page is written by DTU Nanolab  internal''
In 2022, the POCl<sub>3</sub> line on the furnace was modified to make the setup more safe. At the same time some software changes were also made, and the recipes on the furnace were updated.
Afterwards, a phosphorus doping test was made to see, if the modification had affected the phosphorus doping process. The test was done with a test wafer and four dummy wafers (two dummy wafers on each side of the test wafers) in the furnace.
====Process:====
* RCA cleaning of the test wafer (p-type, 1-20 Ωcm) and the dummy wafers
* Phosphorus pre-deposition in the Phosphorus Pre-dep furnace (A4).
** Recipe: "POCL900"
** Temperature: 900 °C
** Time: 15 min phosphorus pre-dep and 20 min annealing/N<sub>2</sub> post purge
* BHF dip in the RCA cleaning bench to remove phosphorus glass from the test wafer
* Measure sheet resistance using the 4-point proble
====Results:====
After the process describe above, the sheet resistance on the test wafer was measured.
The sheet resistance was 54 Ωsq in the center of the wafer and 45-48 Ωsq in the edge of the wafer. This correspond quite good to the results that previously had been obtained for the furnace as can be seen on this LabAdviser page.
====Notes about the POCL recipes====
A new recipe for POCL doping called was made, after the POCl<sub>3</sub> line was modified. The N<sub>2</sub> high flow (3 SLM) is on all the time through the recipe. There is a 2 min pre-purge with first N2 low (150 sccm) through the POCl3 bubbler, i.e. with the valves v4a and v4b closed, and then with O2 (0.50 SLM), before the pre-deposition time starts. After the pre-deposition, an N2 low post-purge (500 sccm) is done for 2 minutes with v4a and v4b closed.
 
For safety reasons it is important that the POCl<sub>3</sub> is completely removed from the furnace, before it is opened to load or unload wafers.
With 150 sccm N2 low through 25°C POCl<sub>3</sub> liquid + 3 slm N<sub>2</sub> high + 0.5 slm O<sub>2</sub>, 3300 ppm Cl<sub>2</sub> is created in the tube. These 3300 ppm Cl<sub>2</sub> must be diluted to less than 0.5 ppm (the TLV value).
The tube diameter is 16 cm and the length without ball valve is about 125 cm, and thus the volume is about 25 L. After the phosphorus pre-deposition step, the N<sub>2</sub> high flow (3 SLM) is on during the annealing/N<sub>2</sub> post purge, the cooling and a waiting step. The time for the waiting step is 30 minutes, so even if the annealing time is set to 0 minutes, and the furnace does not have to cool down, there will still be an N<sub>2</sub> high flow for 30 minutes to remove the POCl<sub>3</sub> from the furnace. The waiting time is the same in the abort recipe that is activated, if the POCL doping recipe is aborted.
The recipe can be modified with other temperatures and names.

Latest revision as of 08:29, 23 May 2024

Feedback to this page: click here


The Phosphorus Predep furnace (A4) can be used for phosphorus pre-deposition of silicon wafers, resulting in n-type doping. In the furnace, the silicon wafers are positioned vertically in a quarts boat.


Test of the Phosphorus Predep furnace

This page is written by DTU Nanolab internal

Purpose

To study the correlation between the temperature for the predeposition process and drive-in of the phosphorus doping in the Phosphorus Predep furnace (A4) at DTU Nanolab.

Experimental setup

20 boron doped device wafers (p-type) were used - Four wafers for each of the five different predeposition temperatures (see table below). In the furnace five dummy wafers were placed on each side of the device wafers. The dummy wafers nearest to the device wafers were changed in-between the runs to minimize doping from these dummy wafers.

Run # Temperature Process time with POCl3 Annealing time in O2 Wafer #
1 850 oC 15 minutes 20 minutes 1, 2, 3, 4
2 900 oC 15 minutes 20 minutes 5, 6, 7, 8
3 950 oC 15 minutes 20 minutes 9, 10, 11, 12
4 1000 oC 15 minutes 20 minuntes 13, 14, 15, 16
5 1050 oC 15 minutes 20 minutes 17, 18, 19, 20

After the predeposition two wafers from each run were taken out to be further processed. These wafers were: 1, 2, 5, 6, 9, 10, 13, 14, 17, 18. These wafers were dipped in BHF to remove the phosphorus glass layer before the drive-in process.

The drive-in process was made in the Phosphorus Drive-in furnace (A3) for all the mentioned wafers at same time. At the drive-in process a dummy wafer was placed in-between the wafers that have been predeposited at different temperatures, so doping from wafer to wafer was minimized. The phosphorus drive-in was done with the process "DRY1050" which is a dry oxidation at 1050 oC for 100 minutes and 20 minutes annealing. At the oxidation the O2 flow was 5 SLM, and the N2 flow for annealing was 3 SLM.

Results

Several measurements were done for the different device wafers. After the predeposition, the thickness of the grown phosphorus glass layer was measured, and the sheet resistance and slice resistivity were measured on the same wafer after a BHF etch.

Measurements after phosphorus predeposition
Ellipsometer (center point only) Four Point Probe
Wafer # Temperature [C] Oxide thickness [nm] Refractive index Sheet resistance [Ωsq] Slice Resistivity [Ωcm]
3 850 27,4 1,4623 311 6,22*10-3
7 900 45,27 1,4622 138,5 4,85*10-3
11 950 61,36 1,4625 16,1 1,29*10-3
15 1000 80,45 1,4624 7,4 0,89*10-3
19 1050 119,37 1,4623 6,6 1,49*10-3

The oxide layer was etch in BHF before the drive-in of the doping with a dry oxidation at 1050 oC for 100 minutes and 20 minutes annealing.

Measurements after phosphorus drive-in
Avg. five point on Filmtek Four Point Probe
Wafer # Temperature [oC] Oxide thickness [nm] Refractive index Sheet resistance [Ωsq] Slice Resistivity [Ωcm]
2 850 110,44 1,4654 189,7 3,79*10-3
6 900 116,28 1,4629 101,6 3,56*10-3
9 950 137,06 1,4604 10,0 0,8*10-3
14 1000 141,46 1,4651 4,72 0,57*10-3
18 1050 139,87 1,4659 3,23 0,73*10-3
Blank Si wafer 110,71 1,46286 - -


Resistivity
Sheet resistance
SIMS Measurement After Pre-dep
SIMS Measurement After Drive-in Process at 1050 oC


Looking at the "SIMS Measurement After Drive-in Process at 1050 oC" graph, it can be seen that the two curves "Pre-dep at 950 oC" and "Pre-dep at 1000 oC" are crossing each other, but according to the theory they should not do that. Only one wafer has been measured so there is not that much statistical data to verify it with.


Test of the Phosphorus Predep furnace

This page is written by DTU Nanolab internal

Purpose

To find the result of a specific process using the Phosphorus Predep furnace (A4) followed by a drive in and oxidating the substrate in the Phosphorus drive in furnace (A3).

Experimental setup

Substrate: p-type Si(100,)

Resistivity: 1-20 Ωcm

Recipe: POCL900

Temperature: 900 °C

Time: 15 min

Anneal: 20 min in N2

After removing the oxide in BHF the wafers were oxidized in Phosphor Drive in Furnace (A3) using DRY1050 at 1050°C for 70 min without further annealing in N2. Results are listed in the table below:

Results

Measurements after phosphorus predeposition
Afer predeposition After Oxidation
Test date Sheet resistance [Ω/sq] Oxide thickness [nm] Sheet resistance [Ω/sq
Aug2012 47.0 93.1 41.8
Jan2013 50.5 91.3 55.6
Aug2013 58.0 91.8 41.8
Jan2014 54.1 93.3 33.8
Jan2015 50.8 94.2 39.4


One wafer from Jan2015 was analyzed with SIMS and the profile is shown on the graph below:

SIMS Measurement After Predeposition, before and after oxidation respectively


Result from GreenBelt, @nanolab,Jan 2015


Test of the Phosphorus Predep furnace

Purpose

To find the doping profile after a specific process flow. The test was made by only performing the high-temperature process step after the pre-deposition step done in the Phosphorus Predep furnace (A4). The subsequently high temperature processes was done by using the Phosphorous drive in furnace (A3) and the Oxide Anneal Furnace (C3).

Experimental setup

Substrate: p-type Si(100,)

Resistivity: 1-20 Ωcm

The total thermal budget for the wafers:

Predeposition in Furnace (A4): POCL1000, 15 min, no further anneal

Wet Oxidation in Furnace (A3): WET1050, 30 min, no further anneal

Anneal in Furnace (C1): ANN1000, 30 min in N2

Wet oxidation in Furnace (C1): WET1050, 30 min, no further anneal

Results

The wafer was analyzed with SIMS and the profile is shown on the graph below:


SIMS Measurement after Phosphorous Predeposition and several oxidations and annealings


Result from Trine Holm Christensen, @Space, Feb. 2015


Phosphorous doping test after hardware and software upgrades

This page is written by DTU Nanolab internal

In 2022, the POCl3 line on the furnace was modified to make the setup more safe. At the same time some software changes were also made, and the recipes on the furnace were updated.

Afterwards, a phosphorus doping test was made to see, if the modification had affected the phosphorus doping process. The test was done with a test wafer and four dummy wafers (two dummy wafers on each side of the test wafers) in the furnace.

Process:

  • RCA cleaning of the test wafer (p-type, 1-20 Ωcm) and the dummy wafers
  • Phosphorus pre-deposition in the Phosphorus Pre-dep furnace (A4).
    • Recipe: "POCL900"
    • Temperature: 900 °C
    • Time: 15 min phosphorus pre-dep and 20 min annealing/N2 post purge
  • BHF dip in the RCA cleaning bench to remove phosphorus glass from the test wafer
  • Measure sheet resistance using the 4-point proble

Results:

After the process describe above, the sheet resistance on the test wafer was measured.

The sheet resistance was 54 Ωsq in the center of the wafer and 45-48 Ωsq in the edge of the wafer. This correspond quite good to the results that previously had been obtained for the furnace as can be seen on this LabAdviser page.

Notes about the POCL recipes

A new recipe for POCL doping called was made, after the POCl3 line was modified. The N2 high flow (3 SLM) is on all the time through the recipe. There is a 2 min pre-purge with first N2 low (150 sccm) through the POCl3 bubbler, i.e. with the valves v4a and v4b closed, and then with O2 (0.50 SLM), before the pre-deposition time starts. After the pre-deposition, an N2 low post-purge (500 sccm) is done for 2 minutes with v4a and v4b closed.

For safety reasons it is important that the POCl3 is completely removed from the furnace, before it is opened to load or unload wafers.

With 150 sccm N2 low through 25°C POCl3 liquid + 3 slm N2 high + 0.5 slm O2, 3300 ppm Cl2 is created in the tube. These 3300 ppm Cl2 must be diluted to less than 0.5 ppm (the TLV value).

The tube diameter is 16 cm and the length without ball valve is about 125 cm, and thus the volume is about 25 L. After the phosphorus pre-deposition step, the N2 high flow (3 SLM) is on during the annealing/N2 post purge, the cooling and a waiting step. The time for the waiting step is 30 minutes, so even if the annealing time is set to 0 minutes, and the furnace does not have to cool down, there will still be an N2 high flow for 30 minutes to remove the POCl3 from the furnace. The waiting time is the same in the abort recipe that is activated, if the POCL doping recipe is aborted.

The recipe can be modified with other temperatures and names.