Specific Process Knowledge/Lithography/Descum: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
No edit summary
 
(4 intermediate revisions by the same user not shown)
Line 1: Line 1:
{{:Specific Process Knowledge/Lithography/authors_generic}}
{{cc-nanolab}}


'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Descum click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Descum click here]'''
Line 23: Line 23:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="left"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
Line 40: Line 40:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="left"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
Line 67: Line 67:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 81: Line 81:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 95: Line 95:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 109: Line 109:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 135: Line 135:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 156: Line 156:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 172: Line 172:


=Plasma Asher 3: Descum=
=Plasma Asher 3: Descum=
'''The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager].'''
The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager] - '''requires login'''


Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time.
Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time.
Line 195: Line 195:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
| ||FW/REV|| C2/C1 || Power
| ||FW/REV|| C2/C1 || Power
Line 223: Line 223:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
| ||FW/REV|| C2/C1 || Oxygen || Pressure
| ||FW/REV|| C2/C1 || Oxygen || Pressure
Line 249: Line 249:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
| ||FW/REV|| C2/C1 || Oxygen || Pressure
| ||FW/REV|| C2/C1 || Oxygen || Pressure

Latest revision as of 13:55, 10 May 2023

The contents on this page, including all images and pictures, was created by DTU Nanolab staff unless otherwise stated.

Feedback to this page: click here

Plasma Asher 1

Descum results plasma asher 1. September 2019

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager - requires login

Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.


Recipe 1:
Note: Plasma asher was cold before use

  • O2 flow: 70 ml/min
  • N2 flow: 70 ml/min
  • Power: 150 W
Ashing time (min) 1 2 5 7 10 10
Etched Thickness (nm) 14.2 16.3 47.6 123.2 854.3 862.1


Recipe 2:
Note: Plasma asher was cold before use

  • O2 flow: 500 ml/min
  • N2 flow: 0 ml/min
  • Power: 500 W
Ashing time (min) 1 2 5 7 10 10
Etched Thickness (nm) - 8.1 32.9 271.1 495.6 446.2


Descum tests on UV resists

Conny Hjort & Jesper Hanberg, September 2021

Descum results plasma asher 1. August 2021

Descum of different resists, AZ5214E, AZ701 MiR and AZ2020 nLOF, on a single 100mm wafer was tested. Wafer was placed vertically in the middle of glass carrier.

Recipe settings:
Note: plasma Asher was cold before use.

  • O2 flow: 70 ml/min
  • N2 flow: 70 ml/min

Power: 150 W

Minor temperature rise during processing was observed, but not more than 5 degrees. Starting chamber pressure was around 0.5 mbar.


1,5 um AZ5214E resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 6,28 102,99 76,92 N/A N/A


1,5 um AZ5214E resist placed horizontally in the carrier:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 63,03 143,32 304,29 372,59 N/A


1,5 um AZ701MiR resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 268,88 199,54 219,03 200,86 292,15


1,5 um AZ 2020nLOF resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 1,68 76,51 169,72 481,96 272,59


Plasma Asher 2

Jitka Urbánková & Jesper Hanberg, December 2019

Descum results plasma asher 2 - recipe 1

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager - requires login

Descum of AZ Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.


recipe 1:

  • O2 flow: 100 ml/min
  • N2 flow: 100 ml/min
  • Power: 150 W
Ashing time (min) 1 2 3 4 6 7 8 9 10 12 14 15 20
Etched Thickness (nm) 8,7 5,1 12,5 6,2 31,8 86,0 25,7 46,8 38,3 49,7 59,4 140,1 360,7
Initial temperature (°C) 28 21 31 21 22 28 25 24 21 24 24 22 22
Descum results plasma asher 2 - recipe 2


recipe 2:

  • O2 flow: 500 ml/min
  • N2 flow: 0 ml/min
  • Power: 200 W
Ashing time (min) 1 2 3 4 5 6 7 8 10 12 15 20
Etched Thickness (nm) 8,1 9,4 16,8 55,2 44,0 47,5 42,5 55,1 85,3 122,4 184,8 305,9
Initial temperature (°C) 22 21 21 22 22 22 21 21 20 21 21 22

A linear time dependence was observed after etching 7 minutes or more (recipe 2).

Plasma Asher 3: Descum

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager - requires login

Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time. The plasma asher is equipped with 2 gaslines: oxygen and nitrogen, but all standard processes use only oxygen (as recommended by Diener).


Ashing of AZ MiR701 resist:
You can use two different descum process developments: you can either change power settings or processing chamber pressure.


Testing different power settings:

Descum results for different power settings

Recipe settings:

  • O2 flow: 5 sccm
  • N2 flow: 0
  • Pressure: 0.2 mbar
  • Power: Varied


Experiment parameters:

FW/REV C2/C1 Power
recipe 1 50/0 52/31 50%
recipe 2 100/0 53/31 100%
recipe 3 20/0 51/34 20%



Testing different pressure settings:

Descum results for different pressure settings

Recipe settings:

  • O2 flow: varied
  • N2 flow: 0
  • Pressure: varied
  • Power: V100% (100 W)


Experiment parameters:

FW/REV C2/C1 Oxygen Pressure
recipe 1 100/0 53/31 5 0,2
recipe 2 100/0 37/38 45 0,8


Ashing of AZ5214E resist:

Descum results for different pressure settings


Recipe settings:

  • O2 flow: varied
  • N2 flow: 0
  • Pressure: varied
  • Power: V100% (100 W)


Experiment parameters:

FW/REV C2/C1 Oxygen Pressure
recipe 1 100/0 53/31 17 0,4
recipe 2 100/0 37/39 45 0,8