Specific Process Knowledge/Lithography/Descum: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
No edit summary
 
(28 intermediate revisions by the same user not shown)
Line 1: Line 1:
{{cc-nanolab}}
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Descum click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Descum click here]'''
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page-->


[[Category: Equipment |Lithography descum]]
[[Category: Equipment|Lithography descum]]
[[Category: Lithography|Descum]]
[[Category: Lithography|Descum]]


==Descum results==
__TOC__


=Plasma asher 1=
=Plasma Asher 1=
[[image:Descum Results aug 2019.png|right|frame|400x400px| Descum results plasma asher 1. September 2019]]
[[File:Descum Results aug 2019.png|640px|thumb|right|Descum results plasma asher 1. September 2019]]


'''The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=44 LabManager].'''
The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=55 LabManager] - '''requires login'''


Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.
Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.
Line 22: Line 23:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="left"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
Line 39: Line 40:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="left"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
|'''Ashing time (min)'''|| 1|| 2 || 5 || 7 || 10 || 10   
|-  
|-  
|'''Etched Thickness (nm)'''|| || 8.1 || 32.9 || 271.1 || 495.6 || 446.2
|'''Etched Thickness (nm)'''|| - || 8.1 || 32.9 || 271.1 || 495.6 || 446.2
|-
|-
|}
|}
|}
|}
<br clear="all" />
==Descum tests on UV resists==
''Conny Hjort & Jesper Hanberg, September 2021''
[[Image:PA1_descum.jpg|640px|thumb|Descum results plasma asher 1. August 2021]]


Descum of different resists, AZ5214E, AZ701 MiR and AZ2020 nLOF, on a single 100mm wafer was tested. Wafer was placed vertically in the middle of glass carrier.


==Descum tests on various resists==
'''Recipe settings:'''<br>
''Conny Hjort & Jesper Hanberg, September 2019''
Note: plasma Asher was cold before use.
*O2 flow: 70 ml/min
*N2 flow: 70 ml/min
Power: 150 W


[[image:PA1_descum.jpg|right|frameless|400x400px| Different resist descum results plasma asher 1. August 2021]]
Minor temperature rise during processing was observed, but not more than 5 degrees. Starting chamber pressure was around 0.5 mbar.


Descum of different resists, AZ5214E, AZ701 MiR and AZ2020 nLOF, on a single 100mm wafer was tested. Wafer was placed vertically in the middle of glass carrier.
Recipe setting was the same as in previous test in September 2019: 70ml/min O2, 70 ml/min N2, power 150W, different ashing time 1, 2, 3, 5 and 7 min run. Plasma Asher was cold before use, we observed minor temperature rise during processing, but not more than 5 degrees. Starting chambers pressure was around 0, 5 mbar.


'''1,5 um AZ5214E resist'''
'''1,5 um AZ5214E resist:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 70: Line 77:
|}
|}


'''1,5 um AZ5214E resist placed horizontally in the carrier'''
 
'''1,5 um AZ5214E resist placed horizontally in the carrier:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 83: Line 91:
|}
|}


'''1,5 um AZ701MiR resist'''
 
'''1,5 um AZ701MiR resist:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 96: Line 105:
|}
|}


'''1,5 um AZ 2020nLOF resist'''
 
'''1,5 um AZ 2020nLOF resist:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 110: Line 120:
<br clear="all" />
<br clear="all" />


===[http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_2 Plasma asher 2]===
=Plasma Asher 2=
[[image:descum_graf.jpg|right|frame|355x355px|Descum results plasma asher 2 - recipe 1]]
''Jitka Urbánková & Jesper Hanberg, December 2019''
[[image:descum_graf.jpg|640px|thumb|Descum results plasma asher 2 - recipe 1]]
 
The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=200 LabManager] - '''requires login'''


Descum of AZ  Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.
Descum of AZ  Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.


Experiment parameters:
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center"
|- style="background:LightGrey"
| ||O2 flow|| N2 flow || Power
|-
|'''recipe 1''' || 100 || 100 || 150
|-
|'''recipe 2''' || 500 || 0 || 200
|-
|}
|}


 
'''recipe 1:'''
 
*O2 flow: 100 ml/min
'''recipe 1'''
*N2 flow: 100 ml/min
*Power: 150 W
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 146: Line 147:
|}
|}


[[image:graf_descum-recipe2.png|640px|thumb|Descum results plasma asher 2 - recipe 2]]




[[image:graf_descum-recipe2.png|right|frame|355x355px|Descum results plasma asher 2 - recipe 2]]
'''recipe 2:'''
 
*O2 flow: 500 ml/min
'''recipe 2'''
*N2 flow: 0 ml/min
*Power: 200 W
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
   
   
|- style="background:LightGrey"
|- style="background:LightGrey"
Line 165: Line 168:
|}
|}


We can observe linear dependance of etched material on time after etching 7 minutes and more (recipe 2).
A linear time dependence was observed after etching 7 minutes or more (recipe 2).
<br clear="all" />


=Plasma Asher 3: Descum=
The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager] - '''requires login'''


Jitka Urbánková & Jesper Hanberg
Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time.
December 2019
The plasma asher is equipped with 2 gaslines: oxygen and nitrogen, but all standard processes use only oxygen (as recommended by Diener).


<br clear="all" />


===[http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_3: Plasma asher 3]===
'''Ashing of  AZ MiR701 resist:'''<br>
You can use two different descum process developments: you can either change power settings or processing chamber pressure.


Plasma Asher 3 is specially used for control descum process after lithography. Please notice that you only can process one 4 inch wafer or one small sampel at a time.
Machine is equipped with 2 gaslines: oxygen and nitrogen, but all tests run with oxygen as recommended by Diener.


'''Ashing of  AZ MiR701 resist'''
'''Testing different power settings:'''
[[image:AZMIR701_power_settings.png|640px|thumb|Descum results for different power settings]]


You can use different strategy planing your descum: you can change power settings or you can vary chamber pressure during descum.
'''Recipe settings:'''
*O2 flow: 5 sccm
*N2 flow: 0
*Pressure: 0.2 mbar
*Power: Varied


''Testing different power settings''


[[image:AZMIR701_power_settings.png|right|frame|400x400px| Descum results for different power settings]]
'''Experiment parameters:'''
 
Recipe settings:
Kept oxygen and pressure settings constant at Oxygen: 5 sccm under process; Pressure: 0,2mbar and vary power.
 
Experiment parameters:
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
| ||FW/REV|| C2/C1 || Power
| ||FW/REV|| C2/C1 || Power
Line 206: Line 209:
<br clear="all" />
<br clear="all" />


''Testing different pressure settings''


Recipe settings:
'''Testing different pressure settings:'''
Kept power setting constant at Power: 100% and vary oxygen flow during process.
[[image:AZMIR701_pressure_settings.png|640px|thumb|Descum results for different pressure settings]]


[[image:AZMIR701_pressure_settings.png|right|frame|400x400px| Descum results for different pressure settings]]
'''Recipe settings:'''
*O2 flow: varied
*N2 flow: 0
*Pressure: varied
*Power: V100% (100 W)




Experiment parameters:
'''Experiment parameters:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
| ||FW/REV|| C2/C1 || Oxygen || Pressure
| ||FW/REV|| C2/C1 || Oxygen || Pressure
Line 227: Line 233:
|}
|}
|}
|}
<br clear="all" />
<br clear="all" />


'''Ashing of AZ5214E resist'''
'''Ashing of AZ5214E resist:'''
[[image:AZ5214E_pressure_settings.png|640px|thumb|Descum results for different pressure settings]]


[[image:AZ5214E_pressure_settings.png|right|frame|400x400px| Descum results for different pressure settings]]


Recipe settings:
'''Recipe settings:'''
Kept power setting constant at Power: 100% and vary oxygen flow during process.
*O2 flow: varied
*N2 flow: 0
*Pressure: varied
*Power: V100% (100 W)




Experiment parameters:
'''Experiment parameters:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
{| border="1" cellspacing="1" cellpadding="2" align="center"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|- style="background:LightGrey"
|- style="background:LightGrey"
| ||FW/REV|| C2/C1 || Oxygen || Pressure
| ||FW/REV|| C2/C1 || Oxygen || Pressure

Latest revision as of 13:55, 10 May 2023

The contents on this page, including all images and pictures, was created by DTU Nanolab staff unless otherwise stated.

Feedback to this page: click here

Plasma Asher 1

Descum results plasma asher 1. September 2019

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager - requires login

Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.


Recipe 1:
Note: Plasma asher was cold before use

  • O2 flow: 70 ml/min
  • N2 flow: 70 ml/min
  • Power: 150 W
Ashing time (min) 1 2 5 7 10 10
Etched Thickness (nm) 14.2 16.3 47.6 123.2 854.3 862.1


Recipe 2:
Note: Plasma asher was cold before use

  • O2 flow: 500 ml/min
  • N2 flow: 0 ml/min
  • Power: 500 W
Ashing time (min) 1 2 5 7 10 10
Etched Thickness (nm) - 8.1 32.9 271.1 495.6 446.2


Descum tests on UV resists

Conny Hjort & Jesper Hanberg, September 2021

Descum results plasma asher 1. August 2021

Descum of different resists, AZ5214E, AZ701 MiR and AZ2020 nLOF, on a single 100mm wafer was tested. Wafer was placed vertically in the middle of glass carrier.

Recipe settings:
Note: plasma Asher was cold before use.

  • O2 flow: 70 ml/min
  • N2 flow: 70 ml/min

Power: 150 W

Minor temperature rise during processing was observed, but not more than 5 degrees. Starting chamber pressure was around 0.5 mbar.


1,5 um AZ5214E resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 6,28 102,99 76,92 N/A N/A


1,5 um AZ5214E resist placed horizontally in the carrier:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 63,03 143,32 304,29 372,59 N/A


1,5 um AZ701MiR resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 268,88 199,54 219,03 200,86 292,15


1,5 um AZ 2020nLOF resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 1,68 76,51 169,72 481,96 272,59


Plasma Asher 2

Jitka Urbánková & Jesper Hanberg, December 2019

Descum results plasma asher 2 - recipe 1

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager - requires login

Descum of AZ Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.


recipe 1:

  • O2 flow: 100 ml/min
  • N2 flow: 100 ml/min
  • Power: 150 W
Ashing time (min) 1 2 3 4 6 7 8 9 10 12 14 15 20
Etched Thickness (nm) 8,7 5,1 12,5 6,2 31,8 86,0 25,7 46,8 38,3 49,7 59,4 140,1 360,7
Initial temperature (°C) 28 21 31 21 22 28 25 24 21 24 24 22 22
Descum results plasma asher 2 - recipe 2


recipe 2:

  • O2 flow: 500 ml/min
  • N2 flow: 0 ml/min
  • Power: 200 W
Ashing time (min) 1 2 3 4 5 6 7 8 10 12 15 20
Etched Thickness (nm) 8,1 9,4 16,8 55,2 44,0 47,5 42,5 55,1 85,3 122,4 184,8 305,9
Initial temperature (°C) 22 21 21 22 22 22 21 21 20 21 21 22

A linear time dependence was observed after etching 7 minutes or more (recipe 2).

Plasma Asher 3: Descum

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager - requires login

Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time. The plasma asher is equipped with 2 gaslines: oxygen and nitrogen, but all standard processes use only oxygen (as recommended by Diener).


Ashing of AZ MiR701 resist:
You can use two different descum process developments: you can either change power settings or processing chamber pressure.


Testing different power settings:

Descum results for different power settings

Recipe settings:

  • O2 flow: 5 sccm
  • N2 flow: 0
  • Pressure: 0.2 mbar
  • Power: Varied


Experiment parameters:

FW/REV C2/C1 Power
recipe 1 50/0 52/31 50%
recipe 2 100/0 53/31 100%
recipe 3 20/0 51/34 20%



Testing different pressure settings:

Descum results for different pressure settings

Recipe settings:

  • O2 flow: varied
  • N2 flow: 0
  • Pressure: varied
  • Power: V100% (100 W)


Experiment parameters:

FW/REV C2/C1 Oxygen Pressure
recipe 1 100/0 53/31 5 0,2
recipe 2 100/0 37/38 45 0,8


Ashing of AZ5214E resist:

Descum results for different pressure settings


Recipe settings:

  • O2 flow: varied
  • N2 flow: 0
  • Pressure: varied
  • Power: V100% (100 W)


Experiment parameters:

FW/REV C2/C1 Oxygen Pressure
recipe 1 100/0 53/31 17 0,4
recipe 2 100/0 37/39 45 0,8