== The nano1.0 recipe == | == The nano1.0 recipe == | ||
<!-- | {{Template:Author-jmli1}} | ||
<!--Checked for updates on 2/02-2023 - ok/jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
|+ '''Recipe nano1.0''' | |+ '''Recipe nano1.0''' |
Latest revision as of 15:17, 2 February 2023
Feedback to this page: click here
The nano1.0 recipe
Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab
Recipe | Gas | C4F8 38 sccm, SF6 52 sccm |
---|---|---|
Pressure | 4 mTorr, Strike 3 secs @ 15 mTorr | |
Power | 800 W CP, 50 W PP | |
Temperature | 10 degs | |
Hardware | 100 mm Spacers | |
Time | 120 secs | |
Conditions | Run ID | 1801 |
Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
Mask | 1dfhj10 nm zep etched down to 6dgh4 nm |
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
Nominal trench line width | ' | 30 | 60 | 90 | 120 | 150 | Avg | Std |
Etch rates | nm/min | 239 | 281 | 306 | 320 | 328 | 295 | 36 |
Sidewall angle | degs | 93 | 94 | 93 | 92 | 93 | 93 | 1 |
CD loss | nm/edge | -1 | -5 | -11 | -9 | -32 | -11 | 12 |
CD loss foot | nm/edge | -1 | -5 | -11 | -9 | -2 | -5 | 5 |
Bowing | 41 | 33 | 29 | 30 | 22 | 31 | 7 | |
Curvature | -51 | -50 | -43 | -39 | -42 | -45 | 5 | |
zep | nm/min | 46 | ||||||
Comments
The process looks to be too etch aggressive, not enough passivation. Consider any or all of the following:
- Decreasing the wafer temperature (make more passivant)
- Increasing C4F8 flow (make more passivant)
- Increasing platen power (make more directional)
- Decreasing coil power (make less etch-aggressive and more directional.
Also, if the tool has Short Funnel and 5mm spacers fitted, it may be too close to the plasma - previous good nano-scale etch result was achieved with Long Funnel and 100mm spacers.
The conditions are similar to the nano-etch conditions for acceptance process C:
Etch | |
Gas Flow (sccm) | SF6 38 + C4F8 70 |
Pressure (mT) | 4 |
APC angle (%) | 33.2 |
Coil power (W) | 450 |
Matching (Forward/ Load) | L/ 33 & T/ 43 |
HF Platen power (W) | 100 |
Matching (Forward/ Load) | L/ 49 & T/ 53 |
Time | 01:30 |
Hardware configuration | 150mm Long funnel, with baffle & 100mm spacers |
APC Gain | 7.5 (default) |
Platen Temperature | 10°C |
The highlighted sections are the main differences between the Process C conditions Vs new Imprint Trenches conditions: all of the changes would push the process to be more passivant, less etch aggressive and more directional.
Is there any reason why these conditions are not suitable for the Imprint Trenches etch?