Specific Process Knowledge/Etch/DRIE-Pegasus/processA: Difference between revisions
(→10:05) |
(→20:10) |
||
Line 1,173: | Line 1,173: | ||
==20:10== | ==20:10== | ||
{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" | {| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" | ||
Line 1,185: | Line 1,181: | ||
! width="50" rowspan="2"| Process Information | ! width="50" rowspan="2"| Process Information | ||
! colspan="15"| SEM images of trenches | ! colspan="15"| SEM images of trenches | ||
|- | |- | ||
! 2 µm | ! 2 µm | ||
Line 1,203: | Line 1,198: | ||
! 300 µm | ! 300 µm | ||
|- | |- | ||
| January 2013 | |rowspan="2"| January 2013 | ||
| Travka05, 600 nm oxide, '''5% open''' | |rowspan="2"| Travka05, 600 nm oxide, '''5% open''' | ||
| Process A 110 cycles or 20:10 minutes, '''C01549.01''' | |rowspan="2"| Process A 110 cycles or 20:10 minutes, '''C01549.01''' | ||
| [[file:C01549.01 002mu 0129.jpg |75px|frameless ]] | | [[file:C01549.01 002mu 0129.jpg |75px|frameless ]] | ||
| [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]] | | [[file:C01549.01 004-3mu 0128.jpg |75px|frameless ]] | ||
Line 1,221: | Line 1,216: | ||
| [[file:C01549.01 200mu 0118.jpg |75px|frameless ]] | | [[file:C01549.01 200mu 0118.jpg |75px|frameless ]] | ||
| [[file:C01549.01 300mu 0117.jpg |75px|frameless ]] | | [[file:C01549.01 300mu 0117.jpg |75px|frameless ]] | ||
| | |- | ||
|colspan="15"| | |||
{| {{table}} | {| {{table}} | ||
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | | align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | ||
Line 1,254: | Line 1,250: | ||
|} | |} | ||
|- | |- | ||
| January 2013 | |rowspan="2"| January 2013 | ||
| Travka10, 600 nm oxide, '''10% open''' | |rowspan="2"| Travka10, 600 nm oxide, '''10% open''' | ||
| Process A 110 cycles or 20:10 minutes, '''C01549.02''' | |rowspan="2"| Process A 110 cycles or 20:10 minutes, '''C01549.02''' | ||
| [[file:C01549.02 002mu 0085.jpg |75px|frameless ]] | | [[file:C01549.02 002mu 0085.jpg |75px|frameless ]] | ||
| [[file:C01549.02 003mu 0084.jpg |75px|frameless ]] | | [[file:C01549.02 003mu 0084.jpg |75px|frameless ]] | ||
Line 1,272: | Line 1,268: | ||
| [[file:C01549.02 200mu 0072.jpg |75px|frameless ]] | | [[file:C01549.02 200mu 0072.jpg |75px|frameless ]] | ||
| [[file:C01549.02 300mu 0071.jpg |75px|frameless ]] | | [[file:C01549.02 300mu 0071.jpg |75px|frameless ]] | ||
| | |- | ||
|colspan="15"| | |||
{| {{table}} | {| {{table}} | ||
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | | align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | ||
Line 1,305: | Line 1,302: | ||
|} | |} | ||
|- | |- | ||
| January 2013 | |rowspan="2"| January 2013 | ||
| Travka20, 600 nm oxide, '''20% open''' | |rowspan="2"| Travka20, 600 nm oxide, '''20% open''' | ||
| Process A 110 cycles or 20:10 minutes, '''C01549.03''' | |rowspan="2"| Process A 110 cycles or 20:10 minutes, '''C01549.03''' | ||
| [[file:C01549.03 002mu 0087.jpg |75px|frameless ]] | | [[file:C01549.03 002mu 0087.jpg |75px|frameless ]] | ||
| [[file:C01549.03 003mu 0088.jpg |75px|frameless ]] | | [[file:C01549.03 003mu 0088.jpg |75px|frameless ]] | ||
Line 1,323: | Line 1,320: | ||
| [[file:C01549.03 200mu 0100.jpg |75px|frameless ]] | | [[file:C01549.03 200mu 0100.jpg |75px|frameless ]] | ||
| [[file:C01549.03 300mu 0101.jpg |75px|frameless ]] | | [[file:C01549.03 300mu 0101.jpg |75px|frameless ]] | ||
| | |- | ||
|colspan="15"| | |||
{| {{table}} | {| {{table}} | ||
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' | | align="center" style="background:#f0f0f0;"|'''Trench width (µm)''' |
Revision as of 11:54, 21 January 2022
Feedback to this page: click here
Effects on Process A of showerhead change in December 2014
The effects of changing of the showerhead in December 2014 was investigated. Patterned wafers were processed before and after and the profile of the etched features were inspected in SEM. Click on the numbers in the 'Runs' column below to see the profiles.
Recipe | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
Process A | Step1 11 cyc | 20 | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 90>>150 | 0 | 350(1.5s) 550 | 5 | 2800 | 120>>140(1.5s) 45 | Old | 1 | |
Step2 44 cyc | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 150 | 0 | 350(1.5s) 550 | 5 | 2800 | 140(1.5s) 45 | |||||
Step1 11 cyc | 20 | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 90>>150 | 0 | 350(1.5s) 550 | 5 | 2800 | 120>>140(1.5s) 45 | New | 1 | Profile improved | |
Step2 44 cyc | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 150 | 0 | 350(1.5s) 550 | 5 | 2800 | 140(1.5s) 45 |
Process A acceptance test
Process A is labelled Large trench (80μm wide) 150μm depth. In the acceptance test the process was run on a 150 mm SPTS wafer with 12-13 % etch load.
Parameter | Specification | Average result |
---|---|---|
Etch rate (µm/min) | > 15 | 18.9 |
Etched depth (µm) | 150 | 189.1 |
Scallop size (nm) | < 800 | 718 |
Profile (degs) | 91 +/- 1 | 91.1 |
Selectivity to AZ photoresist | > 150 | 310 |
Undercut (µm) | <1.5 | 0.84 |
Uniformity (%) | < 3.5 | 3.0 |
Repeatability (%) | <4 | 0.43 |
Process A parameters | ||||
---|---|---|---|---|
Step 1 | Step 2 | |||
Parameter | Etch | Dep | Etch | Dep |
Gas flow (sccm) | SF6 350 (1.5 s) 550 | C4F8 200 | SF6 350 (1.5 s) 550 | C4F8 200 |
Cycle time (secs) | 7.0 | 4.0 | 7.0 | 4.0 |
Pressure (mtorr) | 25 (1.5 s) 90 >> 150 | 25 | 25 (1.5 s) 150 | 25 |
Coil power (W) | 2800 | 2000 | 2800 | 2000 |
Platen power (W) | 120 >> 140 (1.5) 45 | 0 | 140 (1.5) 45 | 0 |
Cycles | 11 (keep fixed) | 44 (vary this) | ||
Common | Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers |
Quality control procedure
Quality Control (QC) for DRIE-Pegasus | |||||||||||||||||
|
Process A guidelines
Process A is optimized for speed and depending on feature size and etch load it will achieve etch rates up to 25-30 µm/min.
This aggressive etch has a few drawbacks - one of which is the release of energy in the etch process. In general, it is clear that
- The higher the etch rate, the higher rate of released energy.
- The larger an area of silicon is exposed to plasma and hence etched, the higher rate of released energy.
Given its high etch rate, Process A is very sensible to high etch load processes and substrates with reduced cooling efficiency. Therefore, users are generally advised to
- Use Process A with precaution at high etch loads - above some 50%.
- Avoid using Process A on bonded wafers, in particular if the etch load is more than 5-10%. The bonding reduces the heat conduction across the wafer interface so the top wafer will immediately heat up and cause the mask to erode and the bonding polymer to melt.
If you have a bonded sandwich of wafers with very poor heat conduction (typically caused by intermediate polymer layers thicker than a few microns) you are advised to use other etch processes, maybe the deepetch on the ASE.
Process A performance
The perfomance of Process A has been investigated as a function of feature size and etch load.
Experiment
A number of wafers are patterned with the Travka mask set in AZ photoresist or 600 nm oxide. The wafers are then etched (batch recipe with 5 minute TDESC interstep cleans) using two different durations of process A in the DRIE-Pegasus.
|
|
Results: Optical images
- Optical images of the C01548 batch that is processed 10:05 mins.
- Without pre-etch measurements of the thicknesses of the photoresist it is not possible to determine the resist etch rate. However, it looks very uniform.
- Optical images of the C01549 batch that is processed 20:10 mins.
The etching of silicon releases energy. This means that the faster the etch is, the more heat needs to be dissipated. The consequence is the same if a larger percentage of the wafer is etched. Process A is the fastest etch and as seen above, the exposed area plays an important role. As the exposed area increases the oxide mask erosion is more and more pronounced.
If a larger area is to be etched, the cooling must be made more efficient, either by lowering the platen temperature or with increasing the pressure of He on the backside of the wafer. This will be investigated soon.
Results: Etched depths in trenches of different widths
- Graphs
Results: SEM images of trench cross sections
Date | Substrate Information | Process Information | SEM images of trenches | Numbers | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
2 µm | 3 µm | 4 µm | 6 µm | 8 µm | 10 µm | 15 µm | 25 µm | 40 µm | 50 µm | 75 µm | 100 µm | 150 µm | 200 µm | 300 µm | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka05, 600 nm oxide, 5% open | Process A 110 cycles or 20:10 minutes, C01549.01 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka10, 600 nm oxide, 10% open | Process A 110 cycles or 20:10 minutes, C01549.02 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka20, 600 nm oxide, 20% open | Process A 110 cycles or 20:10 minutes, C01549.03 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka35, 600 nm oxide, 35% open | Process A 110 cycles or 20:10 minutes, C01549.04 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
|
10:05
Date | Substrate Information | Process Information | SEM images of trenches | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
2 µm | 3 µm | 4 µm | 6 µm | 8 µm | 10 µm | 15 µm | 25 µm | 40 µm | 50 µm | 75 µm | 100 µm | 150 µm | 200 µm | 300 µm | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka05, AZ 5214, 5% open | Process A 55 cycles or 10:05 minutes, C01548.01 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka10, AZ 5214, 10% open | Process A 55 cycles or 10:05 minutes, C01548.02 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka20, AZ 5214, 20% open | Process A 55 cycles or 10:05 minutes, C01548.03 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka35, AZ 5214, 35% open | Process A 55 cycles or 10:05 minutes, C01548.04 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka50, AZ 5214, 50% open | Process A 55 cycles or 10:05 minutes, C01548.05 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
|
20:10
Date | Substrate Information | Process Information | SEM images of trenches | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
2 µm | 3 µm | 4 µm | 6 µm | 8 µm | 10 µm | 15 µm | 25 µm | 40 µm | 50 µm | 75 µm | 100 µm | 150 µm | 200 µm | 300 µm | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka05, 600 nm oxide, 5% open | Process A 110 cycles or 20:10 minutes, C01549.01 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka10, 600 nm oxide, 10% open | Process A 110 cycles or 20:10 minutes, C01549.02 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka20, 600 nm oxide, 20% open | Process A 110 cycles or 20:10 minutes, C01549.03 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
January 2013 | Travka35, 600 nm oxide, 35% open | Process A 110 cycles or 20:10 minutes, C01549.04 | ![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
![]() |
|