Specific Process Knowledge/Lithography/Espacer: Difference between revisions

From LabAdviser
Tigre (talk | contribs)
No edit summary
Lgpe (talk | contribs)
No edit summary
 
(20 intermediate revisions by 3 users not shown)
Line 1: Line 1:
We have Espacer in stock and approved for use in the cleanroom. You can find a guideline for a process flow here: [[media:Process_Flow_ZEP_ESPACER.docx‎|Process_Flow_ZEP_ESPACER.docx‎]]. Technical information of Espacer can be found here: [[media:Espacer_300_Technical_Info.pdf‎|Espacer_300_Technical_Info.pdf‎]], [[media:Espacer_catalog.pdf‎|Espacer_catalog.pdf‎]].
Espacer is a chemical that works as a discharging layer when e-beam writing on a non-conducting substrate or more than 500nm of dielectric material in on the top surface, this includes resists; it is spun onto the wafer on top of the resist and easily rinsed off the wafer after e-beam exposure.


Please contact [mailto:lithography@danchip.dtu.dk Lithography] if you wish to test this material.
 
All substrates are grounded to the e-beam cassette when properly loaded. On a non-conducting substrate, the accumulation of charges in the substrates will however destroy the e-beam patterning. To avoid this, a charge dissipating layer is added on top of the e-beam resist; this will provide a conducting layer for the electrons to escape, while high-energy electrons will pass through the layer to expose the resist.
 
 
We have Espacer in stock and approved for use in the cleanroom. You can find a guideline for a process flow here: [[media:Process Flow CSAR + ESPACER.docx‎|Process Flow CSAR + ESPACER.docx‎]]. Technical information of Espacer can be found here: [[media:Espacer_300_Technical_Info.pdf‎|Espacer_300_Technical_Info.pdf‎]], [[media:Espacer_catalog.pdf‎|Espacer_catalog.pdf‎]].
 
Espacer is a dirty chemical, so we recommend Electra92, or best Thermal Al eg. 20 nm instead
 
Please contact [mailto:lithography@danchip.dtu.dk Lithography] if you wish to use this material.




Line 12: Line 20:
!No ESPACER
!No ESPACER
!ESPACER
!ESPACER
|-
|-
|-style="background:WhiteSmoke; text-align:center; color:black"
|Wafer
|colspan="2"| Borofloat 4" wafers (JB456), no pretreatment
|-
|-


Line 29: Line 43:
|ESPACER
|ESPACER
|
|
|1 min @ 2000 rpm (no softbake), [[Specific Process Knowledge/Lithography/Coaters#Manual Spinner 1 (Laurell)|Manual Spinner 1 (Laurell)]]
|1 min @ 2000 rpm (no softbake), [[Specific_Process_Knowledge/Lithography/Coaters#Manual_Spin_Coaters|Spin Coater: Manual All Puropse]]
|-
|-


Line 35: Line 49:
|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|E-beam exposure
|E-beam exposure
|colspan="2"|2 nA, aperture 5, dose 150-310 muC/cm2, SHOT A,10
|colspan="2"|2 nA, aperture 5, dose 150-310 muC/cm2, SHOT (A,10)
|-
|-


Line 55: Line 69:
|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|Characterization
|Characterization
|colspan="2"|
|colspan="2"|Nikon ECLIPSE optical microscope, E-5
|-
|-


|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|Nikon ECLIPSE optical microscope, E-5
|All doses
|[[File:NoESPACERoverview2.png|300px]]
|[[File:NoEspacerOverview.png|300px]]
|[[File:ESPACERoverview.png|300px]]
|[[File:ESPACERoverview.png|300px]]
|-
|-


|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|Nikon ECLIPSE optical microscope, E-5
|230 muC/cm2
|[[File:NoESPACERbasedose.png|300px]]
|[[File:NoEspacerOverviewBasedose.png|300px]]
|[[File:ESPACERbasedose.png|300px]]
|[[File:ESPACERbasedose.png|300px]]
|-
|-


|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|Nikon ECLIPSE optical microscope, E-5
|219 muC/cm2
|[[File:noESPACERbasedose+5%.png|300px]]
|[[File:noEspacerBasedose-5%.png|300px]]
|
|
|-
|-


|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|Sputter Coated
|
|
|<10nm Pt at DTU CEN
|-
|-style="background:WhiteSmoke; text-align:center; color:black"
|Characterization
|
|
|Sputter Coated with <10nm Pt at DTU CEN
|Zeiss SEM supra 60VP, D-2
 
|-
|-


|-style="background:WhiteSmoke; text-align:center; color:black"
|-style="background:WhiteSmoke; text-align:center; color:black"
|Zeiss SEM supra 60VP, E-3
|230 muC/cm2
|
|
|[[File:EspacerBorofloat30nmBasedose.png|300px]]
| [[File:EspacerBorofloat30nmBasedose.png|300px]]
|-
|-



Latest revision as of 12:33, 20 August 2021

Espacer is a chemical that works as a discharging layer when e-beam writing on a non-conducting substrate or more than 500nm of dielectric material in on the top surface, this includes resists; it is spun onto the wafer on top of the resist and easily rinsed off the wafer after e-beam exposure.


All substrates are grounded to the e-beam cassette when properly loaded. On a non-conducting substrate, the accumulation of charges in the substrates will however destroy the e-beam patterning. To avoid this, a charge dissipating layer is added on top of the e-beam resist; this will provide a conducting layer for the electrons to escape, while high-energy electrons will pass through the layer to expose the resist.


We have Espacer in stock and approved for use in the cleanroom. You can find a guideline for a process flow here: Process Flow CSAR + ESPACER.docx‎. Technical information of Espacer can be found here: Espacer_300_Technical_Info.pdf‎, Espacer_catalog.pdf‎.

Espacer is a dirty chemical, so we recommend Electra92, or best Thermal Al eg. 20 nm instead

Please contact Lithography if you wish to use this material.


Process No ESPACER ESPACER
Wafer Borofloat 4" wafers (JB456), no pretreatment
Resist AR-P 6200/2 AllResist E-beam resist
Spin Coat 1 min @ 4000 rpm, softbake 2 min @ 150 degC, thickness ~140nm
ESPACER 1 min @ 2000 rpm (no softbake), Spin Coater: Manual All Puropse
E-beam exposure 2 nA, aperture 5, dose 150-310 muC/cm2, SHOT (A,10)
Rinse Rinsed with hand shower in fumehood, dried with N2 gun
Developing SX-AR 600-54/6 60 sec, 60 sec IPA rinse
Characterization Nikon ECLIPSE optical microscope, E-5
All doses
230 muC/cm2
219 muC/cm2
Sputter Coated <10nm Pt at DTU CEN
Characterization Zeiss SEM supra 60VP, D-2
230 muC/cm2