When running any recipe on the SPTS Pro software, a set of process parameters are recorded (defined in the logging recipe that can be modified like any other recipe) as the process runs. This data can be accessed later by looking up the datalog. During the process itself, one can also activate the 'Trace' to monitor the process parameters in real time. | When running any recipe on the SPTS Pro software, a set of process parameters are recorded (defined in the logging recipe that can be modified like any other recipe) as the process runs. This data can be accessed later by looking up the datalog. During the process itself, one can also activate the 'Trace' to monitor the process parameters in real time. To the left in the figure below, some of the most important process parameters are shown for a process run of the recipe Process A. | ||
Revision as of 18:56, 17 March 2020
Feedback to this page: click here
Process optimization using the Picoscope
The original standard recipes on Pegasus 1 differ in many ways. The second step of one of them is listed below:
Process A Step 2 parameters | ||
---|---|---|
Parameter | Etch | Dep |
Gas flow (sccm) | SF6 350 (1.5 s), 550 | C4F8 200 |
Cycle time (secs) | 7.0 | 4.0 |
Pressure (mtorr) | 25 (1.5 s), 150 | 25 |
Coil power (W) | 2800 | 2000 |
Platen power (W) | 140 (1.5) 45 | 0 |
Common | Temperature 20 degs |
When running any recipe on the SPTS Pro software, a set of process parameters are recorded (defined in the logging recipe that can be modified like any other recipe) as the process runs. This data can be accessed later by looking up the datalog. During the process itself, one can also activate the 'Trace' to monitor the process parameters in real time. To the left in the figure below, some of the most important process parameters are shown for a process run of the recipe Process A.
- 4 cycles of Process A
- 4 cycles of Process D4