Specific Process Knowledge/Etch/DRIE-Pegasus/processA: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
Line 363: Line 363:




{| border="2" cellpadding="0" cellspacing="0" style="text-align:center;"
|+ '''Travkatesting2: Process A run for 55 cycles on travka 5, 10, 20, 35, 50 masks'''
|-
! width="30" rowspan="2" | Date
! width="40" rowspan="2"| Substrate Information
! width="50" rowspan="2"| Process Information
! colspan="15"| SEM images of trenches
! rowspan="2" | Numbers
|-
! 2 µm
! 3 µm
! 4 µm
! 6 µm
! 8 µm
! 10 µm
! 15 µm
! 25 µm
! 40 µm
! 50 µm
! 75 µm
! 100 µm
! 150 µm
! 200 µm
! 300 µm
|-
| January 2013
| Travka05, AZ 5214, '''5% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.01'''
| [[file:C01548.01 002mu0025.jpg |75px|frameless ]]
| [[file:C01548.01 003mu0026.jpg |75px|frameless ]]
| [[file:C01548.01 004mu0024.jpg |75px|frameless ]]
| [[file:C01548.01 006mu0023.jpg |75px|frameless ]]
| [[file:C01548.01 008mu0022.jpg |75px|frameless ]]
| [[file:C01548.01 010mu0021.jpg |75px|frameless ]]
| [[file:C01548.01 015mu0020.jpg |75px|frameless ]]
| [[file:C01548.01 025mu0019.jpg |75px|frameless ]]
| [[file:C01548.01 040mu0018.jpg |75px|frameless ]]
| [[file:C01548.01 050mu0016.jpg |75px|frameless ]]
| [[file:C01548.01 075mu0015.jpg |75px|frameless ]]
| [[file:C01548.01 100mu0014.jpg |75px|frameless ]]
| [[file:C01548.01 150mu0013.jpg |75px|frameless ]]
| [[file:C01548.01 200mu0012.jpg |75px|frameless ]]
| [[file:C01548.01 300mu0011.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||92||106||113||126||136||146||161||181||200||208||222||230||238||243||248
|-
| Av. ER (µm/min)||9,2||10,5||11,2||12,5||13,5||14,4||16,0||18,0||19,9||20,7||22,0||22,8||23,6||24,1||24,6
|-
| Av. ER (nm/cyc)||1679||1918||2054||2294||2473||2648||2933||3299||3641||3786||4038||4184||4324||4409||4507
|-
| Sdewll bowing (%)||0,3%||0,2%||0,2%||0,3%||0,3%||0,2%||0,0%||0,2%||0,2%||-0,3%||0,1%||0,1%||0,2%||0,2%||-0,1%
|-
| Sdewll angle(degs)||90,4||90,3||90,5||90,8||90,6||90,9||91,0||90,9||90,9||91,0||90,9||90,9||91,1||91,2||91,4
|-
| Trench width (µm)||4,8||7,1||7,7||9,7||12,6||14,1||20,0||30,3||46,3||56,4||82,5||107,3||156,9||206,7||308,6
|-
|}
|-
| January 2013
| Travka10, AZ 5214, '''10% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.02'''
|[[file:C01548.02 2mu  0001.jpg |75px|frameless ]]
|[[file:C01548.02 3mu  0002.jpg |75px|frameless ]]
|[[file:C01548.02 4mu  0003.jpg |75px|frameless ]]
|[[file:C01548.02 6mu  0004.jpg |75px|frameless ]]
|[[file:C01548.02 8mu  0005.jpg |75px|frameless ]]
|[[file:C01548.02 010mu0006.jpg |75px|frameless ]]
|[[file:C01548.02 015mu0007.jpg |75px|frameless ]]
|[[file:C01548.02 025mu0008.jpg |75px|frameless ]]
|[[file:C01548.02 040mu0009.jpg |75px|frameless ]]
|[[file:C01548.02 050mu0132.jpg |75px|frameless ]]
|[[file:C01548.02 075mu0133.jpg |75px|frameless ]]
|[[file:C01548.02 100mu 0135.jpg |75px|frameless ]]
|[[file:C01548.02 150mu 0134.jpg |75px|frameless ]]
|[[file:C01548.02 200mu 0136.jpg |75px|frameless ]]
|[[file:C01548.02 300mu 0138.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||90||101||108||121||130||138||152||171||189||198||210||218||228||232||239
|-
| Av. ER (µm/min)||8,9||10,0||10,7||12,0||12,9||13,7||15,1||16,9||18,8||19,6||20,9||21,6||22,6||23,1||23,7
|-
| Av. Scllp hght (nm)||1639||1834||1964||2192||2356||2508||2772||3103||3441||3601||3825||3961||4143||4227||4346
|-
| Sdwall bowing (%)||0,40||0,19||0,25||0,16||0,04||0,12||0,16||-0,18||-0,04||0,00||0,04||-0,08||-0,20||-0,05||-0,05
|-
| Sdwall angle (degs)||90,2||90,3||90,5||90,5||90,6||90,7||90,8||91,1||91,1||91,1||91,1||91,2||91,2||91,3||91,6
|-
| Trench width (µm)||5,2||7,2||8,2||10,9||13,2||15,5||20,6||31,3||46,5||56,1||81,2||107,2||158,9||211,1||306,2
|-
|}
|-
| January 2013
| Travka20, AZ 5214, '''20% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.03'''
| [[file:C01548.03 002mu0041.jpg |75px|frameless ]]
| [[file:C01548.03 003mu0040.jpg |75px|frameless ]]
| [[file:C01548.03 004mu0039.jpg |75px|frameless ]]
| [[file:C01548.03 006mu0038.jpg |75px|frameless ]]
| [[file:C01548.03 008mu0037.jpg |75px|frameless ]]
| [[file:C01548.03 010mu0036.jpg |75px|frameless ]]
| [[file:C01548.03 015mu0035.jpg |75px|frameless ]]
| [[file:C01548.03 025mu0034.jpg |75px|frameless ]]
| [[file:C01548.03 040mu0033.jpg |75px|frameless ]]
| [[file:C01548.03 050mu0032.jpg |75px|frameless ]]
| [[file:C01548.03 075mu0031.jpg |75px|frameless ]]
| [[file:C01548.03 100mu0030.jpg |75px|frameless ]]
| [[file:C01548.03 150mu0029.jpg |75px|frameless ]]
| [[file:C01548.03 200mu0028.jpg |75px|frameless ]]
| [[file:C01548.03 300mu0027.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||75||85||92||103||111||117||130||148||164||170||181||188||194||199||203
|-
| Av. ER (µm/min)||7,5||8,4||9,1||10,2||11,0||11,6||12,9||14,7||16,2||16,8||17,9||18,6||19,3||19,7||20,1
|-
| Av. Scllp hght (nm)||1371||1543||1676||1874||2019||2133||2368||2692||2978||3086||3286||3412||3533||3619||3686
|-
| Sdwall bowing (%)||0,46||0,59||0,40||0,42||0,40||0,28||0,35||0,18||0,36||0,36||0,26||0,58||0,40||0,31||0,05
|-
| Sdwall angle (degs)||90,1||90,4||90,4||90,5||90,8||90,6||91,1||91,3||91,4||91,5||91,5||91,7||91,8||91,8||92,2
|-
| Trench width (µm)||4,9||6,1||7,8||10,4||12,2||14,9||19,9||30,5||46,3||57,4||82,3||106,6||158,1||209,0||309,7
|-
|}
|-
| January 2013
| Travka35, AZ 5214, '''35% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.04'''
| [[file:C01548.04 002mu 0042.jpg |75px|frameless ]]
| [[file:C01548.04 003mu 0043.jpg |75px|frameless ]]
| [[file:C01548.04 004mu 0044.jpg |75px|frameless ]]
| [[file:C01548.04 006mu 0046.jpg |75px|frameless ]]
| [[file:C01548.04 008mu 0047.jpg |75px|frameless ]]
| [[file:C01548.04 010mu 0048.jpg |75px|frameless ]]
| [[file:C01548.04 015mu 0049.jpg |75px|frameless ]]
| [[file:C01548.04 025mu 0050.jpg |75px|frameless ]]
| [[file:C01548.04 040mu 0051.jpg |75px|frameless ]]
| [[file:C01548.04 050mu 0052.jpg |75px|frameless ]]
| [[file:C01548.04 075mu 0053.jpg |75px|frameless ]]
| [[file:C01548.04 100mu 0054.jpg |75px|frameless ]]
| [[file:C01548.04 150mu 0055.jpg |75px|frameless ]]
| [[file:C01548.04 200mu 0056.jpg |75px|frameless ]]
| [[file:C01548.04 300mu 0057.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||61||70||76||86||94||100||111||126||139||143||153||158||163||165||168
|-
| Av. ER (µm/min)||6,1||6,9||7,6||8,6||9,3||9,9||11,0||12,5||13,8||14,2||15,2||15,6||16,2||16,4||16,7
|-
| Av. Scllp hght (nm)||1117||1267||1390||1568||1704||1810||2014||2287||2526||2602||2786||2868||2967||3007||3054
|-
| Sdwall bowing (%)||0,22||0,31||0,30||0,46||0,39||0,55||0,41||0,20||-0,04||-0,33||-0,25||-0,19||-0,13||-0,13||-0,21
|-
| Sdwall angle (degs)||89,7||90,1||90,2||90,4||90,5||90,4||90,2||89,9||90,0||89,9||90,2||90,4||90,8||90,9||91,3
|-
| Trench width (µm)||4,5||5,4||6,7||9,0||11,4||13,4||19,1||30,0||45,0||56,2||82,3||108,4||156,3||207,5||308,3
|-
|}
|-
| January 2013
| Travka50, AZ 5214, '''50% open'''
| Process A 55 cycles or 10:05 minutes, '''C01548.05'''
|
| [[file:C01548.05 003mu 0058.jpg |75px|frameless ]]
| [[file:C01548.05 004mu 0059.jpg |75px|frameless ]]
| [[file:C01548.05 006mu 0060.jpg |75px|frameless ]]
| [[file:C01548.05 008mu 0061.jpg |75px|frameless ]]
| [[file:C01548.05 010mu 0062.jpg |75px|frameless ]]
| [[file:C01548.05 015mu 0063.jpg |75px|frameless ]]
| [[file:C01548.05 025mu 0064.jpg |75px|frameless ]]
| [[file:C01548.05 040mu 0065.jpg |75px|frameless ]]
| [[file:C01548.05 050mu 0066.jpg |75px|frameless ]]
| [[file:C01548.05 050mu 0131.jpg |75px|frameless ]]
| [[file:C01548.05 075mu 0067.jpg |75px|frameless ]]
| [[file:C01548.05 100mu 0068.jpg |75px|frameless ]]
| [[file:C01548.05 200mu 0069.jpg |75px|frameless ]]
| [[file:C01548.05 300mu 0070.jpg |75px|frameless ]]
|
{| {{table}}
| align="center" style="background:#f0f0f0;"|'''Trench width (µm)'''
| align="center" style="background:#f0f0f0;"|'''2'''
| align="center" style="background:#f0f0f0;"|'''3'''
| align="center" style="background:#f0f0f0;"|'''4'''
| align="center" style="background:#f0f0f0;"|'''6'''
| align="center" style="background:#f0f0f0;"|'''8'''
| align="center" style="background:#f0f0f0;"|'''10'''
| align="center" style="background:#f0f0f0;"|'''15'''
| align="center" style="background:#f0f0f0;"|'''25'''
| align="center" style="background:#f0f0f0;"|'''40'''
| align="center" style="background:#f0f0f0;"|'''50'''
| align="center" style="background:#f0f0f0;"|'''75'''
| align="center" style="background:#f0f0f0;"|'''100'''
| align="center" style="background:#f0f0f0;"|'''150'''
| align="center" style="background:#f0f0f0;"|'''200'''
| align="center" style="background:#f0f0f0;"|'''300'''
|-
| Etched depth (µm)||||62||67||75||81||86||94||105||113||118||123||125||129||131||133
|-
| Av. ER (µm/min)||||6,2||6,7||7,5||8,0||8,5||9,3||10,4||11,2||11,7||12,2||12,4||12,8||13,0||13,2
|-
| Av. Scllp hght (nm)||||1132||1223||1370||1472||1565||1706||1906||2061||2142||2234||2277||2355||2379||2412
|-
| Sdwall bowing (%)||||0,42||0,61||0,39||0,36||0,41||0,38||0,39||0,52||0,24||0,36||0,47||0,63||0,59||0,32
|-
| Sdwall angle (degs)||||89,9||89,8||90,0||90,1||90,5||90,7||91,1||91,3||91,6||91,8||92,1||92,3||92,4||92,6
|-
| Trench width (µm)||||5,1||6,7||9,3||11,4||13,7||18,6||29,0||44,5||54,4||80,5||106,7||156,9||207,4||310,1
|-
|}
|}


== Process A variations May-June 2016 ==
== Process A variations May-June 2016 ==

Revision as of 13:09, 26 June 2018

Feedback to this page: click here

Effects on Process A of showerhead change in December 2014

The effects of changing of the showerhead in December 2014 was investigated. Patterned wafers were processed before and after and the profile of the etched features were inspected in SEM. Click on the numbers in the 'Runs' column below to see the profiles.


Recipe Name Temp. Deposition step Etch step Comments
Time Pres. C4F8 SF6 O2 Coil Time Pres. C4F8 SF6 O2 Coil Platen Showerhead Runs Key words
Process A Step1 11 cyc 20 4 25 200 0 0 2000 7.0 25(1.5s) 90>>150 0 350(1.5s) 550 5 2800 120>>140(1.5s) 45 Old 1
Step2 44 cyc 4 25 200 0 0 2000 7.0 25(1.5s) 150 0 350(1.5s) 550 5 2800 140(1.5s) 45
Step1 11 cyc 20 4 25 200 0 0 2000 7.0 25(1.5s) 90>>150 0 350(1.5s) 550 5 2800 120>>140(1.5s) 45 New 1 Profile improved
Step2 44 cyc 4 25 200 0 0 2000 7.0 25(1.5s) 150 0 350(1.5s) 550 5 2800 140(1.5s) 45


Process A acceptance test

Process A is labelled Large trench (80μm wide) 150μm depth. In the acceptance test the process was run on a 150 mm SPTS wafer with 12-13 % etch load.

Process A specifications
Parameter Specification Average result
Etch rate (µm/min) > 15 18.9
Etched depth (µm) 150 189.1
Scallop size (nm) < 800 718
Profile (degs) 91 +/- 1 91.1
Selectivity to AZ photoresist > 150 310
Undercut (µm) <1.5 0.84
Uniformity (%) < 3.5 3.0
Repeatability (%) <4 0.43


Process A parameters
Step 1 Step 2
Parameter Etch Dep Etch Dep
Gas flow (sccm) SF6 350 (1.5 s) 550 C4F8 200 SF6 350 (1.5 s) 550 C4F8 200
Cycle time (secs) 7.0 4.0 7.0 4.0
Pressure (mtorr) 25 (1.5 s) 90 >> 150 25 25 (1.5 s) 150 25
Coil power (W) 2800 2000 2800 2000
Platen power (W) 120 >> 140 (1.5) 45 0 140 (1.5) 45 0
Cycles 11 (keep fixed) 44 (vary this)
Common Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers

Quality control procedure

Quality Control (QC) for DRIE-Pegasus
QC Recipe: Process A
Step 1: 11 cycles Step 2: 44 cycles
QC limits DRIE-Pegasus
Etch rate in Si 21 - 28 µm/min
Non-uniformity 2  %

Process A guidelines

Process A is optimized for speed and depending on feature size and etch load it will achieve etch rates up to 25-30 µm/min.

This aggressive etch has a few drawbacks - one of which is the release of energy in the etch process. In general, it is clear that

  1. The higher the etch rate, the higher rate of released energy.
  2. The larger an area of silicon is exposed to plasma and hence etched, the higher rate of released energy.

Given its high etch rate, Process A is very sensible to high etch load processes and substrates with reduced cooling efficiency. Therefore, users are generally advised to

  1. Use Process A with precaution at high etch loads - above some 50%.
  2. Avoid using Process A on bonded wafers, in particular if the etch load is more than 5-10%. The bonding reduces the heat conduction across the wafer interface so the top wafer will immediately heat up and cause the mask to erode and the bonding polymer to melt.

If you have a bonded sandwich of wafers with very poor heat conduction (typically caused by intermediate polymer layers thicker than a few microns) you are advised to use other etch processes, maybe the deepetch on the ASE.

Process A performance

The perfomance of Process A has been investigated as a function of feature size and etch load.

Experiment

A number of wafers are patterned with the Travka mask set in AZ photoresist or 600 nm oxide. The wafers are then etched (batch recipe with 5 minute TDESC interstep cleans) using two different durations of process A in the DRIE-Pegasus.

Wafers
Wafer number Mask Mask material Process A duration
C01548.01 Travka 05 AZ photoresist 55 cycles, 10:05 mins
C01548.02 Travka 10 AZ photoresist 55 cycles, 10:05 mins
C01548.03 Travka 20 AZ photoresist 55 cycles, 10:05 mins
C01548.04 Travka 35 AZ photoresist 55 cycles, 10:05 mins
C01548.05 Travka 50 AZ photoresist 55 cycles, 10:05 mins
Wafers
Wafer number Mask Mask material Process A duration
C01549.01 Travka 05 600 nm oxide 110 cycles, 20:10 mins
C01549.02 Travka 10 600 nm oxide 110 cycles, 20:10 mins
C01549.03 Travka 20 600 nm oxide 110 cycles, 20:10 mins
C01549.04 Travka 35 600 nm oxide 110 cycles, 20:10 mins

Results: Optical images

The etching of silicon releases energy. This means that the faster the etch is, the more heat needs to be dissipated. The consequence is the same if a larger percentage of the wafer is etched. Process A is the fastest etch and as seen above, the exposed area plays an important role. As the exposed area increases the oxide mask erosion is more and more pronounced.

If a larger area is to be etched, the cooling must be made more efficient, either by lowering the platen temperature or with increasing the pressure of He on the backside of the wafer. This will be investigated soon.


Results: Etched depths in trenches of different widths


Travkatesting2: Process A run for 55 cycles on travka 5, 10, 20, 35, 50 masks
Date Substrate Information Process Information SEM images of trenches Numbers
2 µm 3 µm 4 µm 6 µm 8 µm 10 µm 15 µm 25 µm 40 µm 50 µm 75 µm 100 µm 150 µm 200 µm 300 µm
January 2013 Travka05, AZ 5214, 5% open Process A 55 cycles or 10:05 minutes, C01548.01 C01548.01 002mu0025.jpg C01548.01 003mu0026.jpg C01548.01 004mu0024.jpg C01548.01 006mu0023.jpg C01548.01 008mu0022.jpg C01548.01 010mu0021.jpg C01548.01 015mu0020.jpg C01548.01 025mu0019.jpg C01548.01 040mu0018.jpg C01548.01 050mu0016.jpg C01548.01 075mu0015.jpg C01548.01 100mu0014.jpg C01548.01 150mu0013.jpg C01548.01 200mu0012.jpg C01548.01 300mu0011.jpg
Trench width 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 92 106 113 126 136 146 161 181 200 208 222 230 238 243 248
Av. ER (µm/min) 9,2 10,5 11,2 12,5 13,5 14,4 16,0 18,0 19,9 20,7 22,0 22,8 23,6 24,1 24,6
Av. ER (nm/cyc) 1679 1918 2054 2294 2473 2648 2933 3299 3641 3786 4038 4184 4324 4409 4507
Sdewll bowing (%) 0,3% 0,2% 0,2% 0,3% 0,3% 0,2% 0,0% 0,2% 0,2% -0,3% 0,1% 0,1% 0,2% 0,2% -0,1%
Sdewll angle(degs) 90,4 90,3 90,5 90,8 90,6 90,9 91,0 90,9 90,9 91,0 90,9 90,9 91,1 91,2 91,4
Trench width (µm) 4,8 7,1 7,7 9,7 12,6 14,1 20,0 30,3 46,3 56,4 82,5 107,3 156,9 206,7 308,6
January 2013 Travka10, AZ 5214, 10% open Process A 55 cycles or 10:05 minutes, C01548.02 C01548.02 2mu 0001.jpg C01548.02 3mu 0002.jpg C01548.02 4mu 0003.jpg C01548.02 6mu 0004.jpg C01548.02 8mu 0005.jpg C01548.02 010mu0006.jpg C01548.02 015mu0007.jpg C01548.02 025mu0008.jpg C01548.02 040mu0009.jpg C01548.02 050mu0132.jpg C01548.02 075mu0133.jpg C01548.02 100mu 0135.jpg C01548.02 150mu 0134.jpg C01548.02 200mu 0136.jpg C01548.02 300mu 0138.jpg
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 90 101 108 121 130 138 152 171 189 198 210 218 228 232 239
Av. ER (µm/min) 8,9 10,0 10,7 12,0 12,9 13,7 15,1 16,9 18,8 19,6 20,9 21,6 22,6 23,1 23,7
Av. Scllp hght (nm) 1639 1834 1964 2192 2356 2508 2772 3103 3441 3601 3825 3961 4143 4227 4346
Sdwall bowing (%) 0,40 0,19 0,25 0,16 0,04 0,12 0,16 -0,18 -0,04 0,00 0,04 -0,08 -0,20 -0,05 -0,05
Sdwall angle (degs) 90,2 90,3 90,5 90,5 90,6 90,7 90,8 91,1 91,1 91,1 91,1 91,2 91,2 91,3 91,6
Trench width (µm) 5,2 7,2 8,2 10,9 13,2 15,5 20,6 31,3 46,5 56,1 81,2 107,2 158,9 211,1 306,2
January 2013 Travka20, AZ 5214, 20% open Process A 55 cycles or 10:05 minutes, C01548.03 C01548.03 002mu0041.jpg C01548.03 003mu0040.jpg C01548.03 004mu0039.jpg C01548.03 006mu0038.jpg C01548.03 008mu0037.jpg C01548.03 010mu0036.jpg C01548.03 015mu0035.jpg C01548.03 025mu0034.jpg C01548.03 040mu0033.jpg C01548.03 050mu0032.jpg C01548.03 075mu0031.jpg C01548.03 100mu0030.jpg C01548.03 150mu0029.jpg C01548.03 200mu0028.jpg C01548.03 300mu0027.jpg
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 75 85 92 103 111 117 130 148 164 170 181 188 194 199 203
Av. ER (µm/min) 7,5 8,4 9,1 10,2 11,0 11,6 12,9 14,7 16,2 16,8 17,9 18,6 19,3 19,7 20,1
Av. Scllp hght (nm) 1371 1543 1676 1874 2019 2133 2368 2692 2978 3086 3286 3412 3533 3619 3686
Sdwall bowing (%) 0,46 0,59 0,40 0,42 0,40 0,28 0,35 0,18 0,36 0,36 0,26 0,58 0,40 0,31 0,05
Sdwall angle (degs) 90,1 90,4 90,4 90,5 90,8 90,6 91,1 91,3 91,4 91,5 91,5 91,7 91,8 91,8 92,2
Trench width (µm) 4,9 6,1 7,8 10,4 12,2 14,9 19,9 30,5 46,3 57,4 82,3 106,6 158,1 209,0 309,7
January 2013 Travka35, AZ 5214, 35% open Process A 55 cycles or 10:05 minutes, C01548.04 C01548.04 002mu 0042.jpg C01548.04 003mu 0043.jpg C01548.04 004mu 0044.jpg C01548.04 006mu 0046.jpg C01548.04 008mu 0047.jpg C01548.04 010mu 0048.jpg C01548.04 015mu 0049.jpg C01548.04 025mu 0050.jpg C01548.04 040mu 0051.jpg C01548.04 050mu 0052.jpg C01548.04 075mu 0053.jpg C01548.04 100mu 0054.jpg C01548.04 150mu 0055.jpg C01548.04 200mu 0056.jpg C01548.04 300mu 0057.jpg
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 61 70 76 86 94 100 111 126 139 143 153 158 163 165 168
Av. ER (µm/min) 6,1 6,9 7,6 8,6 9,3 9,9 11,0 12,5 13,8 14,2 15,2 15,6 16,2 16,4 16,7
Av. Scllp hght (nm) 1117 1267 1390 1568 1704 1810 2014 2287 2526 2602 2786 2868 2967 3007 3054
Sdwall bowing (%) 0,22 0,31 0,30 0,46 0,39 0,55 0,41 0,20 -0,04 -0,33 -0,25 -0,19 -0,13 -0,13 -0,21
Sdwall angle (degs) 89,7 90,1 90,2 90,4 90,5 90,4 90,2 89,9 90,0 89,9 90,2 90,4 90,8 90,9 91,3
Trench width (µm) 4,5 5,4 6,7 9,0 11,4 13,4 19,1 30,0 45,0 56,2 82,3 108,4 156,3 207,5 308,3
January 2013 Travka50, AZ 5214, 50% open Process A 55 cycles or 10:05 minutes, C01548.05 C01548.05 003mu 0058.jpg C01548.05 004mu 0059.jpg C01548.05 006mu 0060.jpg C01548.05 008mu 0061.jpg C01548.05 010mu 0062.jpg C01548.05 015mu 0063.jpg C01548.05 025mu 0064.jpg C01548.05 040mu 0065.jpg C01548.05 050mu 0066.jpg C01548.05 050mu 0131.jpg C01548.05 075mu 0067.jpg C01548.05 100mu 0068.jpg C01548.05 200mu 0069.jpg C01548.05 300mu 0070.jpg
Trench width (µm) 2 3 4 6 8 10 15 25 40 50 75 100 150 200 300
Etched depth (µm) 62 67 75 81 86 94 105 113 118 123 125 129 131 133
Av. ER (µm/min) 6,2 6,7 7,5 8,0 8,5 9,3 10,4 11,2 11,7 12,2 12,4 12,8 13,0 13,2
Av. Scllp hght (nm) 1132 1223 1370 1472 1565 1706 1906 2061 2142 2234 2277 2355 2379 2412
Sdwall bowing (%) 0,42 0,61 0,39 0,36 0,41 0,38 0,39 0,52 0,24 0,36 0,47 0,63 0,59 0,32
Sdwall angle (degs) 89,9 89,8 90,0 90,1 90,5 90,7 91,1 91,3 91,6 91,8 92,1 92,3 92,4 92,6
Trench width (µm) 5,1 6,7 9,3 11,4 13,7 18,6 29,0 44,5 54,4 80,5 106,7 156,9 207,4 310,1

Process A variations May-June 2016

Process A may overpassivate producing grass. To investigate the results


Recipe Temp. Deposition step Etch step Comments
Time Pres. C4F8 Coil Time Pressure SF6 O2 Coil Platen SEM images Key words
PrA-0 20 4 25 200 2000 7.0 25(1.5s) 150 350(1.5s) 550 5 2800 140(1.5s) 45 4 Step 2 original recipe
PrA-1 20 3.5 25 200 2000 7.0 25(1.5s) 150 350(1.5s) 550 5 2800 140(1.5s) 45 4 Shorter dep cycle
PrA-2 20 4 25 150 2000 7.0 25(1.5s) 150 350(1.5s) 550 5 2800 140(1.5s) 45 4 Lower C4F8 flow in dep cycle


Process Log entries