Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessD/NewProcessD: Difference between revisions
Created page with " {| border="2" cellpadding="0" cellspacing="0" style="text-align:center;" |+ '''Process runs''' |- ! rowspan="2" width="40"| Date ! colspan="4" width="120"| Substrate Informat..." |
No edit summary |
||
Line 17: | Line 17: | ||
! width="40" | Comments | ! width="40" | Comments | ||
|- | |- | ||
| | | 15/12-2014 | ||
| 4" Wafer with AZ resist | | 4" Wafer with AZ resist | ||
| Travka50 pattern | | Travka50 pattern | ||
| Si / 50 | | Si / 50 % | ||
| Pegasus/jmli | | Pegasus/jmli | ||
| | | 20 minute TDESC clean | ||
| danchip/jml/showerhead/prD | | danchip/jml/showerhead/prD/New Process D, 75 cycles or 5:00 minutes | ||
| S004743 | |||
| | |||
! New showerhead | ! New showerhead | ||
| | | | ||
[[file:S00743-01.jpg|150px|frameless]] | |||
[[file:S00743-02.jpg|150px|frameless]] | |||
[[file:S00743-03.jpg|150px|frameless]] | |||
[[file:S00743-04.jpg|150px|frameless]] | |||
[[file:S00743-05.jpg|150px|frameless]] | |||
[[file:S00743-06.jpg|150px|frameless]] | |||
[[file:S00743-06.jpg|150px|frameless]] | |||
[[file:S00743-07.jpg|150px|frameless]] | |||
|- | |- | ||
|} | |} |
Revision as of 15:50, 16 January 2015
Date | Substrate Information | Process Information | SEM Images | ||||||
---|---|---|---|---|---|---|---|---|---|
Wafer info | Mask | Material/ Exposed area | Tool / Operator | Conditioning | Recipe | Wafer ID | Comments | ||
15/12-2014 | 4" Wafer with AZ resist | Travka50 pattern | Si / 50 % | Pegasus/jmli | 20 minute TDESC clean | danchip/jml/showerhead/prD/New Process D, 75 cycles or 5:00 minutes | S004743 | New showerhead |
File:S00743-01.jpg File:S00743-02.jpg File:S00743-03.jpg File:S00743-04.jpg File:S00743-05.jpg File:S00743-06.jpg File:S00743-06.jpg File:S00743-07.jpg |