Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange: Difference between revisions
Jump to navigation
Jump to search
Line 79: | Line 79: | ||
! width="100" | Key words | ! width="100" | Key words | ||
|- | |- | ||
! rowspan="7" | | ! rowspan="7" | Process A <!-- recipe name --> | ||
! | ! Step 1 <!-- step --> | ||
| | | 20 <!-- chiller temp --> | ||
! | ! 4 <!-- dep time --> | ||
| | | 25 <!-- dep pressure --> | ||
| | | 200 <!-- C4F8 flow --> | ||
| 0 <!-- SF6 flow --> | | 0 <!-- SF6 flow --> | ||
| 0 <!-- O2 flow --> | | 0 <!-- O2 flow --> | ||
| | | 2000 <!-- coil power --> | ||
| | | 7.0 <!-- etch time --> | ||
| | | 25(1.5s) 90>>150 <!-- etch pressure --> | ||
| | | 0 <!-- C4F8 flow --> | ||
| | | 350(1.5s) 550 <!-- SF6 flow --> | ||
| 5 <!-- O2 flow --> | | 5 <!-- O2 flow --> | ||
| | | 2800 <!-- coil power --> | ||
| | | 120>>140(1.5s) 45 <!-- platen power --> | ||
! Old <!-- Showerhead --> | ! Old <!-- Showerhead --> | ||
| [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ | | [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange/ProcessA | 1]] <!-- link processes --> | ||
| | | <!-- keywords --> | ||
|- | |- | ||
| polySi etch DUV mask <!-- step --> | | polySi etch DUV mask <!-- step --> |
Revision as of 10:29, 16 December 2014
Comparison of continuous processes
Process | Before | After | |||||
---|---|---|---|---|---|---|---|
Name/Type | Description | Wafer ID | Comment | SEM images | Wafer ID | Comment | SEM images |
Continuous black silicon recipe on blank wafer | 15 mins, -10 degrees, 32 mtorr, 60 sccm SF6, 55 sccm O2, 70 W platen | S004592 | Wafer centre | ![]() |
S004679 | Wafer centre | ![]() |
S004592 | Wafer edge | ![]() |
S004679 | Wafer edge | ![]() | ||
S00XXX | 8" wafer | S00XXX | Wafer centre | File:S00XX centre.jpg | |||
S00XXXx | Wafer edge | File:S00XXX dge.jpg | S00XXX | Wafer edge | File:S00xxxx edge.jpg |
Comparison of switched processes
Recipe description | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
Process A | Step 1 | 20 | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 90>>150 | 0 | 350(1.5s) 550 | 5 | 2800 | 120>>140(1.5s) 45 | Old | 1 | |
polySi etch DUV mask | 30 | 2.3 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
Cpoly1 | 30 | 1.2 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | Very aggressive, unusable | |
Cpoly2 | 30 | 1.4 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
Cpoly3 | 30 | 1.6 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
Cpoly4 | 30 | 1.8 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
Cpoly5 | 30 | 2.0 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 |
Recipe description | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
Polysilicon etch | polySi etch DUV mask | 30 | 2.3 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | Old | 1 | Slightly over-etching to ensure complete absence of grass |
polySi etch DUV mask | 30 | 2.3 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
Cpoly1 | 30 | 1.2 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | Very aggressive, unusable | |
Cpoly2 | 30 | 1.4 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
Cpoly3 | 30 | 1.6 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
Cpoly4 | 30 | 1.8 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||