Specific Process Knowledge/Thermal Process/Dope with Phosphorus: Difference between revisions
No edit summary |
No edit summary |
||
Line 2: | Line 2: | ||
The Phosphorus Predep furnace (A4) can be used for predeposition of silicon wafers with phosphorus | The Phosphorus Predep furnace (A4) can be used for predeposition of silicon wafers with phosphorus, resulting in N-type doping. In the furnace, the silicon wafers are positioned in a quarts boat. | ||
''' | ''' | ||
Line 17: | Line 17: | ||
====Experimental setup==== | ====Experimental setup==== | ||
''' | ''' | ||
20 boron doped wafers (p-type) | 20 boron doped wafers (p-type) were used - Four wafers for each of the five different predeposition temperatures. In the furnace five dummy wafers were placed on each side of the processed wafers. The dummy wafer nearest to the test wafers were changed in-between the runs to miniminze doping from this dummy wafer. | ||
{| border="1" cellspacing="1" cellpadding="2" style="text-align:center;" width="690" ||3||4||5 | {| border="1" cellspacing="1" cellpadding="2" style="text-align:center;" width="690" ||3||4||5 | ||
Line 33: | Line 33: | ||
|} | |} | ||
''' | ''' | ||
After the | After the predeposition two wafers from each run were taken out to be further processed. These wafers were: 1, 2, 5, 6, 9, 10, 13, 14, 17, 18. | ||
These wafers | These wafers were dipped in BHF to remove the phosphorus glass layer before the drive-in process. The drive-in process was made in the Phosphorus Drive-in furnace (A3). At the drive-in process a dummy wafer was placed in-between the wafers from different temperatures so doping from wafer to wafer was minimized. The drive-in was done with the process "DRY1050" with is a dry oxidation at 1050 <sup>o</sup>C for 100 minutes and 20 minutes annealing. At the oxidation was the O<sub>2</sub> flow was 5 SLM, and the N<sub>2</sub> flow for annealing was 3 SLM. | ||
====Result==== | ====Result==== | ||
''' | ''' | ||
Several measurements were done for the different wafers in the process. After the pre-deposition thickness of the Phosphorus glass layer was measured and the sheet resistance and slice resistivity measured on the same wafer after a BHF etch. | |||
{| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" | {| border="2" cellpadding="2" cellspacing="1" style="text-align:center;" |
Revision as of 10:21, 21 October 2013
Feedback to this page: click here
The Phosphorus Predep furnace (A4) can be used for predeposition of silicon wafers with phosphorus, resulting in N-type doping. In the furnace, the silicon wafers are positioned in a quarts boat.
Test of the Phosphorus Predep furnace
Purpose
To study the coherence between the temperature for the predeposition process and drive-in of the doping with phosphorus in the Phosphorus Predep furnace (A4) at DTU Danchip.
Experimental setup
20 boron doped wafers (p-type) were used - Four wafers for each of the five different predeposition temperatures. In the furnace five dummy wafers were placed on each side of the processed wafers. The dummy wafer nearest to the test wafers were changed in-between the runs to miniminze doping from this dummy wafer.
Run # | Temperature | Process time with POCl3 | Anneal time in N2 | Wafer # |
---|---|---|---|---|
1 | 850 oC | 15 minutes | 20 miuntes | 1, 2, 3, 4 |
2 | 900 oC | 15 minutes | 20 miuntes | 5, 6, 7, 8 |
3 | 950 oC | 15 minutes | 20 miuntes | 9, 10, 11, 12 |
4 | 1000 oC | 15 minutes | 20 miuntes | 13, 14, 15, 16 |
5 | 1050 oC | 15 minutes | 20 miuntes | 17, 18, 19, 20 |
After the predeposition two wafers from each run were taken out to be further processed. These wafers were: 1, 2, 5, 6, 9, 10, 13, 14, 17, 18.
These wafers were dipped in BHF to remove the phosphorus glass layer before the drive-in process. The drive-in process was made in the Phosphorus Drive-in furnace (A3). At the drive-in process a dummy wafer was placed in-between the wafers from different temperatures so doping from wafer to wafer was minimized. The drive-in was done with the process "DRY1050" with is a dry oxidation at 1050 oC for 100 minutes and 20 minutes annealing. At the oxidation was the O2 flow was 5 SLM, and the N2 flow for annealing was 3 SLM.
Result
Several measurements were done for the different wafers in the process. After the pre-deposition thickness of the Phosphorus glass layer was measured and the sheet resistance and slice resistivity measured on the same wafer after a BHF etch.
Ellipsometer (center point only) | Four Point Probe | ||||
---|---|---|---|---|---|
Wafer # | Temperature [C] | Thinkness [nm] | Refrative index | Sheet resistance [Ωsq] | Slice Resistivity [Ωcm] |
3 | 850 | 27,4 | 1,4623 | 311 | 17,32 |
7 | 900 | 45,27 | 1,4622 | 138,5 | 7,61 |
11 | 950 | 61,36 | 1,4625 | 16,12 | 0,859 |
15 | 1000 | 80,45 | 1,4624 | 7,4 | 0,392 |
19 | 1050 | 119,37 | 1,4623 | 6,6 | 0,246 |
Avg. five point on Filmtek | Four Point Probe | ||||
---|---|---|---|---|---|
Wafer # | Temperature [C] | Thinkness [nm] | Refrative index | Sheet resistance [Ωsq] | Slice Resistivity [Ωcm] |
2 | 850 | 110,44 | 1,4654 | 189,7 | 13,06 |
6 | 900 | 116,28 | 1,4629 | 101,6 | 5,32 |
9 | 950 | 137,06 | 1,4604 | 10,05 | 0,527 |
14 | 1000 | 141,46 | 1,4651 | 4,72 | 0,216 |
18 | 1050 | 139,87 | 1,4659 | 3,23 | 0,165 |
Test | 110,71 | 1,46286 | - | - |
Looking at the 'SIMS Measurement after Drive-in Process at 1050 C' it can be seen that 'Pre-dep at 950 C' and 'Pre-dep at 1000 C' are crossing each other but they should not do that. There have only been meassured on one wafer so there is not that mush statistical data to verify it with.