Line 19: Line 19:
|}
|}


Resulting resist thickness can be determined as y = ax<sup>b</sup>, where y is thickness, x is spin speed, a = 11664 and b = -0.442.
Resulting resist thickness can be determined as y = ax<sup>b</sup>, where y is thickness [nm], x is spin speed [RPM], a = 11664 and b = -0.442.

Revision as of 12:59, 22 January 2024

AR-P 617 is a positive PMMA based E-beam resist from Allresist. Process information provided by Allresist can be found here.

Spin coating

AR-P 617 can be spin coated on LabSpin 2 and 3 using the CSAR/PMMA bowlset. A spin curve for AR-P 617.06 is provided below. Process parameters are:

  • Date: January 22nd 2024
  • Coater: LabSpin 3
  • Substrate: 2" Si
  • Acceleration: 1000 RPM/s
  • Time: 60 s
  • Baking temperature: 200C (setpoint at 222C)
  • Baking time: 120 s
ARP617SpinCurve.png

AR-P 617.06 spin curve.

Resulting resist thickness can be determined as y = axb, where y is thickness [nm], x is spin speed [RPM], a = 11664 and b = -0.442.