Specific Process Knowledge/Etch/Etching of Titanium: Difference between revisions
No edit summary |
|||
Line 25: | Line 25: | ||
|- | |- | ||
|'''Chemical solution''' | |'''Chemical solution''' | ||
|HF:NH< | |HF:NH<sub>4</sub>F | ||
|NH< | |NH<sub>3</sub>OH:H<sub>2</sub>O<sub>2</sub>:H<sub>2</sub>O - 1:1:5 | ||
|- | |- | ||
|'''Process temperature''' | |'''Process temperature''' | ||
Line 66: | Line 66: | ||
|- | |- | ||
|} | |} | ||
== Dry etching of titanium == | == Dry etching of titanium == | ||
See the [[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal Etch]] page. | See the [[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal Etch]] page. |
Revision as of 15:31, 18 October 2012
Ething of Titanium can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done either with ICP using Chlorine chemistry or with IBE by sputtering with Ar ions.
Wet etching of Titanium
We have two solutions for wet titanium etching:
- BHF
- Cold RCA1
Do it by making your own set up in a beaker in a fume hood - preferably in cleanroom 2 or 4. BHF etching can also take place in the PP-etch bath in the fume hood in cleanroom 2.
Comparing the two solutions
BHF | Cold RCA1 | |
---|---|---|
General description | Etch of titanium with or without photoresist mask. | Etch of titanium (as stripper or with eagle resist). |
Chemical solution | HF:NH4F | NH3OH:H2O2:H2O - 1:1:5 |
Process temperature | Room temperature | Room temperature |
Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
Eagle resist |
Etch rate |
Not known (it bubbles while etching) |
Not known |
Batch size |
1-5 4" in beaker 1-25 wafers at a time in PP-etch bath |
1-5 4" wafer at a time |
Etch bath | Beaker or PP-etch bath in the fume hood in cleanroom 2. | Beaker |
Allowed materials |
No restrictions when used in beaker or PP-etch bath in the fume hood in cleanroom 2. Make a note on the beaker of which materials have been processed. |
No restrictions when used in beaker. Make a note on the beaker of which materials have been processed. |
Dry etching of titanium
See the ICP Metal Etch page.