Line 334: |
Line 334: |
| |<!--'''Date'''--> 25/01<br>-2024 | | |<!--'''Date'''--> 25/01<br>-2024 |
| |<!--'''SEM picture'''--> [[File:25.01 CHF3.t2 45w 15m-01.png|250px]] [[File:25.01 CHF3.t2 45w 15m-02.png|250px]] [[File:25.01 CHF3.t2 45w 15m-03.png|250px]] [[File:25.01-CHF3.t2-45w-15m-04.png|250px]] <br> *it's visible that redeposits, so the ER and selectivity may not be correct. | | |<!--'''SEM picture'''--> [[File:25.01 CHF3.t2 45w 15m-01.png|250px]] [[File:25.01 CHF3.t2 45w 15m-02.png|250px]] [[File:25.01 CHF3.t2 45w 15m-03.png|250px]] [[File:25.01-CHF3.t2-45w-15m-04.png|250px]] <br> *it's visible that redeposits, so the ER and selectivity may not be correct. |
| |<!--'''Etch rate in SiO2'''-->250nm- 9,18 <br> <br>500nm- 28,03 <br> <br>1000nm- 28,03 <br> <br>2000nm- 28,75 | | |<!--'''Etch rate in SiO2'''-->250nm- 9,18 <br> <br>500nm- 22,46 <br> <br>1000nm- 28,03 <br> <br>2000nm- 28,75 |
| |<!--'''Etch rate in resist'''-->250nm- 11,09 <br> <br>500nm- 4,22 <br> <br>1000nm- 4,22 <br> <br>2000nm- 4,40 | | |<!--'''Etch rate in resist'''-->250nm- 11,09 <br> <br>500nm- 3,96 <br> <br>1000nm- 4,22 <br> <br>2000nm- 4,40 |
| |<!--'''Selectivity (SiO2:resist)'''-->250nm- 0,83 <br> <br>500nm- 6,64 <br> <br>1000nm- 6,64 <br> <br>2000nm- 6,5 | | |<!--'''Selectivity (SiO2:resist)'''-->250nm- 0,83 <br> <br>500nm- 5,67 <br> <br>1000nm- 6,64 <br> <br>2000nm- 6,5 |
| |- | | |- |
| |- | | |- |
Revision as of 14:45, 22 April 2024
Tests performed with UV resist:
The tests were performed on a 100mm wafer patterned on MLA3, with 2.2um AZ5214E resist.
Recipe
|
Recipe parameters
|
Duration (min)
|
Date
|
SEM picture
|
Redeposition - top view
|
Profile angles
|
Etch rate in SiO2
|
Etch rate in resist (AZ5214E inverse)
|
Selectivity (SiO2:resist)
|
CHF3_t1
|
CHF3= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
12:00
|
04/09/2023
|
|
|
|
69.7 nm/min +/- 10.5%
|
57.3 nm/min +/- 12.9%
|
1.22
|
CHF3_t2
|
CHF3= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
25:00
|
04/09/2023
|
|
|
|
26.7 nm/min +/- 11.9%
|
24.2 nm/min +/- 21.1%
|
1.1
|
CHF3 t2
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
9,7 nm/min +/- 34.4%
|
1,8 nm/min +/- 46.5%
|
5.4
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 10 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
12/09/2023
|
|
|
|
59,6 nm/min +/- 12.9%
|
47,5 nm/min +/- 21.5%
|
1.25
|
CHF3_t1
|
CHF3= 22.5 sccm O2= 10 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
11/09/2023
|
|
|
|
60,6 nm/min +/- 10.1%
|
130,8 nm/min +/- 8.8%
|
0.46
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
20/09/2023
|
|
|
|
47,3 nm/min +/- 12%
|
26,4 nm/min +/- 17,4%
|
1.8
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 35 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
36,5 nm/min +/- 10.6%
|
17,5 nm/min +/- 13.9%
|
2.09
|
CHF3 t1
|
CHF3= 35 sccm H2= 35 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
42 nm/min +/- 15.4%
|
23,8 nm/min +/- 22.2%
|
1.76
|
CHF3 t1
|
CHF3= 22.5 sccm CF4= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
75,8 nm/min +/- 13.1%
|
74,9 nm/min +/- 10.8%
|
1.01
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 25mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
-
|
-
|
no etch done, polymer deposited
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 0°C
|
10:00
|
22/09/2023
|
|
|
|
48 nm/min +/- 11.2%
|
23,3 nm/min +/- 13.7%
|
2.06
|
Tests performed with DUV resist:
The resist used was a negative DUV resist (UVN) with 915nm + 88nm BARC layer.
Recipe
|
Recipe parameters
|
Duration (min)
|
Date
|
SEM picture
|
Etch rate in SiO2
|
Etch rate in resist (UVN)
|
Selectivity (SiO2:resist)
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 30W Press= 2.5mTorr Temp= 20°C
|
10:00
|
13/11/23
|
|
47
|
24.6
|
1.9
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
10:00
|
13/11/23
|
|
59
|
30
|
1.9
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 45W Press= 2.5mTorr Temp= 0°C
|
10:00
|
07/12/23
|
|
96
|
56
|
1.7
|
CHF3_t2
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
10:00
|
23/10/23
|
|
27
|
12,5
|
2.1
|
CHF3_t2
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
20:00
|
23/10/23
|
|
8.15
|
7.5
|
1.1
|
25 jan 2024 - SiO2 test
CHF3_t2 @ 45W platen, 15min
|
Values
|
SEM pictures
|
Comments
|
Structure size (nm)
|
structure pitch (nm)
|
SiO2 ER (nm/min)
|
Resist ER (nm/min)
|
Selectivity SiO2/resist
|
|
|
250
|
500
|
9.18
|
11.09
|
0.83
|
|
|
500
|
1000
|
22.46
|
3.96
|
5.67
|
|
*it's visible that redeposits, so the ER and selectivity may not be correct
|
1000
|
2000
|
28.03
|
4.22
|
6.64
|
|
*
|
2000
|
4000
|
28.75
|
4.40
|
6.5
|
|
*
|
Recipe
|
Time (min)
|
Date
|
SEM picture
|
Etch rate SiN (nm/min)
|
Etch rate resist (nm/min)
|
Selectivity (SiN:resist)
|
CHF3_t1 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 30W Press= 2.5mTorr Temp= 20°C
|
10:00
|
25/01 -2024
|
|
250nm- 61,99 500nm- 68,12 1000nm- 74,7 2000nm- 76,55
|
250nm- 61,31 500nm- 49,85 1000nm- 46,83 2000nm- 47,3
|
250nm- 1,01 500nm- 1,37 1000nm- 1,6 2000nm- 1,62
|
CHF3_t1 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
10:00
|
25/01 -2024
|
|
250nm- 90,74 500nm- 84,63 1000nm- 89,33 2000nm- 94,34
|
250nm- 81,1 500nm- 53,77 1000nm- 52,23 2000nm- 54,81
|
250nm- 1,12 500nm- 1,57 1000nm- 1,71 2000nm- 1,72
|
CHF3_t2 CF4= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
15:00
|
25/01 -2024
|
*it's visible that redeposits, so the ER and selectivity may not be correct.
|
250nm- 9,18 500nm- 22,46 1000nm- 28,03 2000nm- 28,75
|
250nm- 11,09 500nm- 3,96 1000nm- 4,22 2000nm- 4,40
|
250nm- 0,83 500nm- 5,67 1000nm- 6,64 2000nm- 6,5
|
Etch test of Silicon Nitride
Tested on chips (2*2cm)
Recipe
|
Time (min)
|
Date
|
SEM picture
|
Redeposition - top view
|
Etch rate SiN (nm/min)
|
Etch rate resist (nm/min)
|
Selectivity (SiN:resist)
|
CHF3_t1 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
2:30
|
29/02 -2024
|
|
|
250nm- 155,08 500nm- 170,32 1000nm- 174,45 2000nm- 179,76
|
250nm- 65,52 500nm- 56,36 1000nm- 64,56 2000nm- 68,84
|
250nm- 2,37 500nm- 3,02 1000nm- 2,70 2000nm- 2,61
|
CHF3_t2 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
5:00
|
29/02 -2024
|
|
|
250nm- 28,12 500nm- 41,86 1000nm- 66 2000nm- 63,62
|
250nm- 23,26 500nm- 22,60 1000nm- 16,74 2000nm- 15,34
|
250nm- 1.21 500nm- 1.85 1000nm- 3.94 2000nm- 4.15
|
CF4lowCP CF4= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
5:00
|
29/02 -2024
|
|
|
250nm- 76,50 500nm- 73,92 1000nm- 73,94 2000nm- 76,50
|
250nm- 44,98 500nm- 33,52 1000nm- 31,16 2000nm- 25,66
|
250nm- 1,70 500nm- 2,21 1000nm- 2,37 2000nm- 2,98
|