Line 242: |
Line 242: |
| <br clear="all" /> | | <br clear="all" /> |
|
| |
|
| =2SiO2 test - 5 jan 2024= | | =SiO2 test - 5 jan 2024= |
|
| |
|
| Tested on chips (2*2cm). The following results were processed on chips bonded to a 100mm wafer. They were patterned with 915 UVN resist (DUV negative) and 65nm of BARC. The SiO2 layer was 2um (deposited on the C1 furnace).
| | * The SiO2 layer deposited was 2um, deposited on the C1 furnace (recipe: WET1100, 12h40+00:20). |
| | * They were patterned with 915 UVN resist (DUV negative) and 65nm of BARC. |
| | * The following results were processed on chips (2*2cm) bonded to a 100mm dummy wafer. |
| <br> | | <br> |
|
| |
|
Revision as of 15:00, 22 April 2024
Tests performed with UV resist:
The tests were performed on a 100mm wafer patterned on MLA3, with 2.2um AZ5214E resist.
Recipe
|
Recipe parameters
|
Duration (min)
|
Date
|
SEM picture
|
Redeposition - top view
|
Profile angles
|
Etch rate in SiO2
|
Etch rate in resist (AZ5214E inverse)
|
Selectivity (SiO2:resist)
|
CHF3_t1
|
CHF3= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
12:00
|
04/09/2023
|
|
|
|
69.7 nm/min +/- 10.5%
|
57.3 nm/min +/- 12.9%
|
1.22
|
CHF3_t2
|
CHF3= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
25:00
|
04/09/2023
|
|
|
|
26.7 nm/min +/- 11.9%
|
24.2 nm/min +/- 21.1%
|
1.1
|
CHF3 t2
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
9,7 nm/min +/- 34.4%
|
1,8 nm/min +/- 46.5%
|
5.4
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 10 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
12/09/2023
|
|
|
|
59,6 nm/min +/- 12.9%
|
47,5 nm/min +/- 21.5%
|
1.25
|
CHF3_t1
|
CHF3= 22.5 sccm O2= 10 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
11/09/2023
|
|
|
|
60,6 nm/min +/- 10.1%
|
130,8 nm/min +/- 8.8%
|
0.46
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
20/09/2023
|
|
|
|
47,3 nm/min +/- 12%
|
26,4 nm/min +/- 17,4%
|
1.8
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 35 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
36,5 nm/min +/- 10.6%
|
17,5 nm/min +/- 13.9%
|
2.09
|
CHF3 t1
|
CHF3= 35 sccm H2= 35 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
42 nm/min +/- 15.4%
|
23,8 nm/min +/- 22.2%
|
1.76
|
CHF3 t1
|
CHF3= 22.5 sccm CF4= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
75,8 nm/min +/- 13.1%
|
74,9 nm/min +/- 10.8%
|
1.01
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 25mTorr Temp= 20°C
|
10:00
|
22/09/2023
|
|
|
|
-
|
-
|
no etch done, polymer deposited
|
CHF3 t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 0°C
|
10:00
|
22/09/2023
|
|
|
|
48 nm/min +/- 11.2%
|
23,3 nm/min +/- 13.7%
|
2.06
|
Tests performed with DUV resist:
The resist used was a negative DUV resist (UVN) with 915nm + 88nm BARC layer.
Recipe
|
Recipe parameters
|
Duration (min)
|
Date
|
SEM picture
|
Etch rate in SiO2
|
Etch rate in resist (UVN)
|
Selectivity (SiO2:resist)
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 30W Press= 2.5mTorr Temp= 20°C
|
10:00
|
13/11/23
|
|
47
|
24.6
|
1.9
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
10:00
|
13/11/23
|
|
59
|
30
|
1.9
|
CHF3_t1
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 45W Press= 2.5mTorr Temp= 0°C
|
10:00
|
07/12/23
|
|
96
|
56
|
1.7
|
CHF3_t2
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
10:00
|
23/10/23
|
|
27
|
12,5
|
2.1
|
CHF3_t2
|
CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 25W Press= 2.5mTorr Temp= 20°C
|
20:00
|
23/10/23
|
|
8.15
|
7.5
|
1.1
|
SiO2 test - 5 jan 2024
- The SiO2 layer deposited was 2um, deposited on the C1 furnace (recipe: WET1100, 12h40+00:20).
- They were patterned with 915 UVN resist (DUV negative) and 65nm of BARC.
- The following results were processed on chips (2*2cm) bonded to a 100mm dummy wafer.
Recipe
|
Time (min)
|
Date
|
SEM picture
|
Etch rate SiN (nm/min)
|
Etch rate resist (nm/min)
|
Selectivity (SiN:resist)
|
CHF3_t1 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 30W Press= 2.5mTorr Temp= 20°C
|
10:00
|
25/01 -2024
|
|
250nm- 61,99 500nm- 68,12 1000nm- 74,7 2000nm- 76,55
|
250nm- 61,31 500nm- 49,85 1000nm- 46,83 2000nm- 47,3
|
250nm- 1,01 500nm- 1,37 1000nm- 1,6 2000nm- 1,62
|
CHF3_t1 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
10:00
|
25/01 -2024
|
|
250nm- 90,74 500nm- 84,63 1000nm- 89,33 2000nm- 94,34
|
250nm- 81,1 500nm- 53,77 1000nm- 52,23 2000nm- 54,81
|
250nm- 1,12 500nm- 1,57 1000nm- 1,71 2000nm- 1,72
|
CHF3_t2 CF4= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
15:00
|
25/01 -2024
|
*it's visible that redeposits, so the ER and selectivity may not be correct.
|
250nm- 9,18 500nm- 22,46 1000nm- 28,03 2000nm- 28,75
|
250nm- 11,09 500nm- 3,96 1000nm- 4,22 2000nm- 4,40
|
250nm- 0,83 500nm- 5,67 1000nm- 6,64 2000nm- 6,5
|
Etch test of Silicon Nitride
- The nitride layer deposited was 560nm, on the PECVD4 (recipe: Standard HF SiN with wafer clean, for 1h).
- They were patterned with 750 DUV resist and 65nm of BARC (exposure:355 J/m2, focus:-3.1).
- The following results were processed on chips (2*2cm) bonded to a 100mm dummy wafer.
Recipe
|
Time (min)
|
Date
|
SEM picture
|
Redeposition - top view
|
Etch rate SiN (nm/min)
|
Etch rate resist (nm/min)
|
Selectivity (SiN:resist)
|
CHF3_t1 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 800W Platen= 15W Press= 2.5mTorr Temp= 20°C
|
2:30
|
29/02 -2024
|
|
|
250nm- 155,08 500nm- 170,32 1000nm- 174,45 2000nm- 179,76
|
250nm- 65,52 500nm- 56,36 1000nm- 64,56 2000nm- 68,84
|
250nm- 2,37 500nm- 3,02 1000nm- 2,70 2000nm- 2,61
|
CHF3_t2 CHF3= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
5:00
|
29/02 -2024
|
|
|
250nm- 28,12 500nm- 41,86 1000nm- 66 2000nm- 63,62
|
250nm- 23,26 500nm- 22,60 1000nm- 16,74 2000nm- 15,34
|
250nm- 1.21 500nm- 1.85 1000nm- 3.94 2000nm- 4.15
|
CF4lowCP CF4= 22.5 sccm H2= 22.5 sccm Coil= 150W Platen= 45W Press= 2.5mTorr Temp= 20°C
|
5:00
|
29/02 -2024
|
|
|
250nm- 76,50 500nm- 73,92 1000nm- 73,94 2000nm- 76,50
|
250nm- 44,98 500nm- 33,52 1000nm- 31,16 2000nm- 25,66
|
250nm- 1,70 500nm- 2,21 1000nm- 2,37 2000nm- 2,98
|