Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using RIE1 or RIE2

From LabAdviser
Jump to navigation Jump to search

RIE (Reactive Ion Etch) can be used for etching silicon oxide. The etch is anisotropic with vertical or angled sidewalls depending on the process recipe and the masking material and geometry. The SiO2 is etched by flour radicals assisted by ion bombardment.

The substrate:

Most be a wafer of 4" or below or small pieces, not higher than about 2mm.

The silicon can be masked by these materials:

  • Photoresist
  • E-beam resist
  • Silicon
  • Silicon Nitride
  • Aluminium
  • Chromium (ONLY RIE2!)
  • Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)

Most used recipes:

Resist as masking material:

Recipe: 1SiO2mre
Masking material Photoresist
CF4 flow 14 sccm
CHF3 flow 26 sccm
Pressure 100 mTorr
RF-power 60 W
Expected results in RIE1 Expected results in RIE2
Etch rate in SiO2 ~20-30 nm/min ~20-30 nm/min
Etch rate in Si3N4 ? ?
Etch rate in P-Si (when used as mask) ~30 nm/min ~30 nm/min
Etch rate in Si

(etching down to Si)

Expected <2 nm/min Expected <2 nm/min

mre:mask resist

PolySilicon as masking material

Recipe: 1SiO2msi
Masking material Silicon
CF4 flow 8 sccm
CHF3 flow 40 sccm
Pressure 150 mTorr
RF-power 150 W
Expected results in RIE1 Expected results in RIE2
Etch rate in SiO2 ~70-80 nm/min ~70-80 nm/min
Etch rate in Si3N4 ? ?
Etch rate in P-Si (when used as mask) ~20-30 nm/min ~20-30 nm/min
Etch rate in Si

(etching down to Si)

? ?

msi:mask silicon

Burned resist as masking material (developed for waveguides by Haiyan Ou @DTU Photonics):

Recipe: 1SiO2mbr
Masking material Burned resist (250oC)
CHF3 flow 84 sccm
Pressure 60 mTorr
RF-power 200 W
Expected results in RIE1 Expected results in RIE2
Etch rate in SiO2 ~120 nm/min ~120 nm/min
Etch rate burned resist ? ?
Etch rate in Si3N4 ? ?
Etch rate in P-Si (when used as mask) ? nm/min ? nm/min
Etch rate in Si

(etching down to Si)

? ?

mbr:mask burned resist

A survey of the parameter space using photoresist as masking material

A DOE has been performed. A short summery is given here: (in progress)

RIE1:

A Design Of Experiment (DOE) has been performed. A screening experiment: full factorial with to levels: 9 different runs and 3 repetitions. Here is a short summary:

The Design of the experiment

Recipe:
Total flow rate (CHF3 flow + CF4 flow) 40 sccm
CHF3 flow rate/Total flow rate 65-75%
Pressure 100-120 mTorr
RF-power 45-65 W

<br\>


Results

Results from a screening experiment should be taken "with a gain of salt" meaning use it only as a rough guide line and test your recipe before use.


Etch rate
Etch rate as a function of power and pressure at 70% CHF3. The etch rate decreases a little as a function of %CHF3.


Selectivity to photoresist

Selectivity as a function of power and pressure at 65% CHF3.
Selectivity as a function of power and pressure at 70% CHF3.
Selectivity as a function of power and pressure at 75% CHF3.


More details on the DOE can be seen here: "DOE RIE1 siliconoxide etch of small structures" (not available yet).