Specific Process Knowledge/Thin film deposition/Deposition of Gold/Roughness of Au
Feedback to this page: click here
Roughness and uniformity of Au layers
Experimental
Au was deposited directly on unprocessed Si wafers (on top of the native oxide), and the deposited layers were thereafter examined with AFM.
The deposition parameters were changed, and different equipment was used. Below, AFM pictures of layers deposited with different parameters can be seen.
Results
Layers from Wordentec
The deposition rate was varied between 1.5 Å/s and 10 Å/s. There are no substential differences of the roughness, for different rates. The differences in height of the tallest and lowest structure of the AFM pictures are in all cases between 4 and 6 nm.
The layer deposited in Wordentec is uniform, without any larger structures. Below a 2.5 x 2.5 µm large area of the surface is shown, the difference in hight between the lowest and tallest structure is about 7nm.