Specific Process Knowledge/Thin film deposition/Deposition of Chromium/Deposition of Chromium

From LabAdviser

Uniformity of Cr layers

Cr have been deposited with both E-beam evaporation and sputtering deposition to examine if there are differences in the uniformity of the Cr layers.

Experimental

Cr depositions have been done directly on unprocessed Si wafers, all depositions has been done in Wordentec. The deposited layers have therafter been examined with AFM.


Results

There are differences in uniformity and grain size, for the various deposition methods. For the sputtering processes there are large differences depending on the settings during the process, i. e. Ar pressure and effect.


E-beam process

The Cr layer deposited with e-beam in the Wordentec has a low roughness, and are uniform. The deposition rate has been 10 Å/s.

E-beam deposited Cr layer; deposited in the Wordentec, rate 10 Å/s.



Sputting prosess

In the Wordentec the Ar pressure can be set to between and mbar during the process, and the effect may be varied between 150 and 400 W.

Here are AFM pictures of sputtered layers, deposited with different settings, shown. (Deposition rates for different setting are listed here: Deposition rate)



Effect 150 W, pressure mbar

With these settings the deposited layers are uniform and has a low roughness.

Sputter deposited Cr layer: settings 150 W and mbar.


Effect 405 W, pressure mbar

405 W and mbar Ar pressure results in a surface with large roughness. The surface grais are comparably small (most about 30 nm in diameter, and almost all below 50 nm).

Sputter deposited Cr layer: settings 405 W and mbar.


Effect 405 W, pressure mbar

These settings give a rough surface, with larger grains (up to 100nm in diameter).

Sputter deposited Cr layer: settings 405 W and mbar.


Conclusions

The roughness of Cr layers is very different for the sputter depositions with different setting. The layer with lowest roughness is achived by using 150 W and mbar argon pressure. A layer with similar rouhgness is also the result of an e-beam process (Wordentec). However, the use of sputtering deposition will give a better step coverage then the e-beam process.


(Please contact Katharina Nilson if you have any questions regarding the study.)