Et2Zn or Zn(CH3CH2)2 = DEZ (diethylzinc)

Recipe: AZO 20T

Maximum deposition thickness: 100 nm

Temperature: 150 oC - 250 oC

# macrocycles n
# cycles 19 1
Precursor DEZ DEZ H2O H2O TMA TMA H2O H2O
Nitrogen flow 150 sccm 150 sccm 200 sccm 200 sccm 150 sccm 150 sccm 200 sccm 200 sccm
Pulse time 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s
Purge time 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s


How to fill out the process log in LabManager:

The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.

DEZ pulse time: (0.1 + 0.1) s * 19 = 3.8 s

TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s

H2O pulse time: [(0.1 + 0.1) s * 19] + [(0.1 + 0.1) s * 1] = 4.0 s

The number of cycles for each precursor now equals the number of macrocycles (n).


Recipe: AZO 25T

Maximum deposition thickness: 100 nm

Temperature: 150 oC - 250 oC

# macrocycles n
# cycles 24 1
Precursor DEZ DEZ H2O H2O TMA TMA H2O H2O
Nitrogen flow 150 sccm 150 sccm 200 sccm 200 sccm 150 sccm 150 sccm 200 sccm 200 sccm
Pulse time 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s
Purge time 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s


How to fill out the process log in LabManager:

The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.

DEZ pulse time: (0.1 + 0.1) s * 24 = 4.8 s

TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s

H2O pulse time: [(0.1 + 0.1) s * 24] + [(0.1 + 0.1) s * 1] = 5.0 s

The number of cycles for each precursor now equals the number of macrocycles (n).


Recipe: AZO 30T

Maximum deposition thickness: 100 nm

Temperature: 150 oC - 250 oC

# macrocycles n
# cycles 29 1
Precursor DEZ DEZ H2O H2O TMA TMA H2O H2O
Nitrogen flow 150 sccm 150 sccm 200 sccm 200 sccm 150 sccm 150 sccm 200 sccm 200 sccm
Pulse time 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s
Purge time 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s

How to fill out the process log in LabManager:

The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.

DEZ pulse time: (0.1 + 0.1) s * 29 = 5.8 s

TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s

H2O pulse time: [(0.1 + 0.1) s * 29] + [(0.1 + 0.1) s * 1] = 6.0 s

The number of cycles for each precursor now equals the number of macrocycles (n).


Recipe: AZO 35T

Maximum deposition thickness: 100 nm

Temperature: 150 oC - 250 oC

# macrocycles n
# cycles 34 1
Precursor DEZ DEZ H2O H2O TMA TMA H2O H2O
Nitrogen flow 150 sccm 150 sccm 200 sccm 200 sccm 150 sccm 150 sccm 200 sccm 200 sccm
Pulse time 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s 0.1 s
Purge time 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s 0.5 s 20.0 s

How to fill out the process log in LabManager:

The pulse time for each precursor equals the total pulse time times the number of cycles in each macrocycle.

DEZ pulse time: (0.1 + 0.1) s * 34 = 6.8 s

TMA pulse time: (0.1 + 0.1 )s * 1 = 0.2 s

H2O pulse time: [(0.1 + 0.1) s * 34] + [(0.1 + 0.1) s * 1] = 7.0 s

The number of cycles for each precursor now equals the number of macrocycles (n).