Striation: Side wall roughness

When etching silicon oxide rough sidewalls are most often seem. This effect is called striation, because it creates stripes along the etched profile. The literature gives several explanations for this. The two main courses seems to be:

  1. deposition on the sidewalls as the etch proceeds, coursing masking effects
    • This can come from flour-carbon polymers from the plasma (some this this layer protects from striation)
    • Re-deposition of sputtered SiO2
  2. damage of the resist mask coursed by plasma heating and/or interaction with the resist. This pattern change at the edge gets transferred to the oxide profile during the etch.
    • Resist edge gets rough during etching due to plasma heating (out-gassing while the surface get UV hardened. This make the resist crumple).
    • The edge can maybe also get roughened due to sputtering.

This work is focused on trying to improve the resist to avoid the resist damage during etching. From a previous test it has been seen that pre baking the resist AZ1452e at 150 degrees for 5 min can prevent the crumpling of the resist, See results HERE. However this makes the resist flow so the edge profile will not remain vertical.

  1. First I characterized how our present three standard resists (AZ5214E, AZ nLof and AZ Mir) looked after an SiO2 etch in the AOE (recipe: SiO2_mres). The characterization was done by
    • SEM: to visually see the SiO2 sidewall roughness and how the resist looks after etch. This only gives a qualitative characterization. See HERE
    • AFM: to get at quantitative value for the resist roughness after the etch. I have seem in the literature that this measure reflects the sidewall roughness of the resist. See HERE
  2. Second we tried to toughen the resist by cross linking (by UV flood exposure after development) and heat treatment. Heat treatment at 110 degrees to effectuate the cross linking and heat treatment at 150 degrees to further out-gas and harden the resist. This was only done to AZ5214E and AZ nLof as AZ MIR?


Sidewall roughness and resist surface after AOE etch viewed with SEM for the three resists: AZ5214E, AZ nLof and AZ MIR

Roughness of the resist after AOE etch measured with the AFM of the three resists: AZ5214E, AZ nLof and AZ MIR

Sidewall roughness/resist surface roughness effected by UV curing and heat treatment of nLof resist Section under construction.jpg

AOE etch with nLof resist with different treatments´
From AFM results from these tests it looks like it does not help to make further UV exposure to nLof resist but it does have some effect to heat it afterwards to 150dg. It has not be explores if this effects the CD. The SEM images does not confirm this improvement, maybe the image quality is not good enough.
  1 2 3 4 5
Treatment No treatment before AOE etch No treatment after 5min AOE etch Flood-E 70s + 1min@110dg 5min@150dg Flood-E 70s + 60s@110dg + 5min@150dg
SEM image NLof0 31.jpg NLof1 1 27.jpg NLof2 0006.jpg NLof3 55.jpg NLof4 67.jpg
AFM roughness scan Ra=2.1nm Rmax=25.1nm NLof0 pre AOE 1 5my.jpg Ra=3.31nm Rmax=28.0nm NLof1 1.jpg Ra=3.34nm Rmax=26.8nm NLof2 pretreat1 2.jpg Ra=2.45nm, Rmax=19.4nm NLof3.jpg Ra=2.52nm, Rmax=23.7nm NLof4.jpg
D D1 D2 D3 D4 D5

Sidewall roughness/resist surface roughness effected by UV curing and heat treatment of AZ5214E resist Section under construction.jpg

AOE etch with AZ5214E resist with different treatments
From AFM results from these tests it looks like it helps to make UV exposure and 110dg heat treatment to AZ5414E resist but it does not have convinving effect to heat it afterwards to 150dg. From the SEM images it is difficult to judge if the wall roughness is less. It does not look like a major difference.
  1 2 3 4
Treatment No treatment before AOE etch No treatment after 5min AOE etch Flood-E 55s + 120s@110dg Flood-E 55s + 120s@110dg + 5min@150dg
SEM image AZ0 14.jpg Az1 1 09.jpg AZ2 0040.jpg Az3 41.jpg
AFM roughness scan Pre etch: cannot measure Ra=4.40nm, Rmax=36.5nm AZ1 4.jpg Ra=3.68nm, Rmax=25.6nm AZ2 4.jpg Ra=3.57nm, Rmax=28.5nm AZ3.jpg
D D1 D2 D3 D4