The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows:
Parameter
|
Recipe name: SiO2_res (SiO2 etch with resist mask)
|
Variations over SiO2_res made in 2010 by BGHE
|
Coil Power [W]
|
1300
|
1000-1600
|
Platen Power [W]
|
200
|
150-300
|
Platen temperature [oC]
|
0
|
0
|
He flow [sccm]
|
174
|
174, 300
|
C4F8 flow [sccm]
|
5
|
5
|
H2 flow [sccm]
|
4
|
0, 4
|
Pressure [mTorr]
|
4
|
2.3, 4
|
Etch rates in different materials using the standard "Silicon oxide etch with resist mask"
Material to be etched
|
Etch rate using SiO2_res
|
Thermal oxide
|
~230nm/min (5% etch load) - etch load dependency see here
|
TEOS oxide (5% load)
|
233nm/min ±0.7% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
|
|
PECVD1 (standard) oxide (5% load)
|
242nm/min ±0.6% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
|
|
Al2O from the ALD
|
50nm can be etched in 10min - etched in November 2014 by FRSTO@danchip
|
|
Silicon rich nitride from furnace B2
|
136nm was etched in 1min (whole wafer) - etched in October 2015 by bghe@danchip
|
|
Using different resist masks: results using the standard recipe for "Silicon oxide etch with resist mask" ![Section under construction.jpg](/images/thumb/9/9a/Section_under_construction.jpg/70px-Section_under_construction.jpg)
.
|
Az
|
MIR
|
nLof
|
KRF
|
CSAR
|
Selectivity to thermal oxide [:1]
|
- 2-3 - etch load dependency see here
- 1.9 - tested November 2015 by BGHE
|
1.8 - tested November 2015 by BGHE
|
2.0 - tested November 2015 by BGHE
|
~2 - tested May 2013 by Christian Østergaard @nanotech.
|
.
|
Profile [o]
|
~90
|
.
|
.
|
.
|
.
|
Roughness of the resist after etch - striation on sidewalls
|
.
|
.
|
.
|
.
|
.
|
Images
|
See here
|
.
|
.
|
See images here
|
.
|
Comments
|
A negative resist process was done to make the mask. I have not had so good results with a positive resist process.
|
.
|
.
|
.
|
Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned and could not be removed by CSAR stripper (AR600-71). For a better recipe look here
|
Striation: Side wall roughness
- Striation with different resists used
Az resist - profile after etch
Mir resist - profile after etch
nLof resist - profile after etch
Variations over the standard "SiO2 etch with resist mask" recipe
Typical results
|
Variations over SiO2_res made in 2010 by BGHE See results here
|
Etch rate of thermal oxide
|
~160-340nm/min
|
Selectivity to AZ resist [:1]
|
2.7-4.3
|
Profile angle
|
83-90
|
Images
|
See here
|
Comments
|
.
|