Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE

From LabAdviser

Feedback to this page: click here


What masking material should I choose when etching SiO2/glass in the AOE?

Photoresist mask - not too deep etches
Etching SiO2 with resist as masking material is the prefered masking material for many purposes. The main reason for using photo resist as masking material is that it is easy and fast to make and easy to remove afterwards. The selectivity of resist to SiO2 is in the range of 3-4.

The main draw back when using photoresist as masking material is heating of the substrate during the etch. SiO2 is a hard material to etch and therefore needs a high DC bias to allow the ion bombardment to be enegetic enough to etch the SiO2. This ion bombardment heats up the surface and even when cooling the platen to zero degrees Celcius the resist mask can exceed 100 degrees Celcius. Combined with the fact that the plasma UV hardens the surface of the resist this can create crumpled resist surface and perforated egdes, see images here. Etching a few microns down in the SiO2 normally does not heat up the resist too much but when etching deeper like 5-10µm there is a large change for getting problems with overheating the resist.


Si/P-Si mask - deeper etches
P-Si is a good masking layer for deeper etches. The selectivity to SiO2 is measured to be better than 1:15. The P-Si on the back side seems to prevent declamping of a APOX substrate during a deep etch on a high load wafer (e.g. 50% load), contrary to using photo resist mask on the APOX substrate. The wafer bow is created when removing part of the top oxide layer due to stress in the oxide layers.

Draw backs: the recipe we have now is giving a high line width reduction (1µm when etching 7.5µm down). Take a look at some recipes and results


Al mask - deeper etches - more redeposition

Al is allowed as masking material but we do not advise it. It can however be useful under some curcumstances. It is expected to have a high selectivity to SiO2 greater than 50.

Draw back: The draw back is that Al does not form any volatile products with the Flour gasses. This means that any Al sputtered of has the chance of getting redeposited on the surface.


Cr mask - deeper etches/high aspect ratio etches where the other materials cannot be used

Cr works well as masking material but due to cross contamination issues we prefer to avoid Cr in the machine. Cr does in contrary to Al form some volatile components with the flour gasses and therefore redeposition problems are not so severe. We do allow Cr as masking material when the other masking materials cannot be used.

So fare it has been found useful for etching nanostructures in quartz substrates.


Etching of micro structures in Silicon Oxide with resist as masking material

Quality Controle (QC) for AOE
QC Recipe: QC mres
C4F8 flow 5 sccm
H2 flow 4 sccm
He flow 174 sccm
Pressure 4 mTorr
Coil power 1300 W
Platen power 200 W
Platen Temperature 20 deg. C
Etch Load 100%
QC limits AOE
Etch rate in SiO2 180 - 195 nm/min
Non-uniformity <2.28 %


Standard silicon oxide etch using resist as masking material

The standard recipe for oxide etching with photo resist as masking material is called: SiO2_res. The parameters and results so fare are as follows:

The standard recipe for etching SiO2 with resist mask

Parameter Recipe name: SiO2_res (SiO2 etch with resist mask) Variations over SiO2_res made in 2010 by BGHE
Coil Power [W] 1300 1000-1600
Platen Power [W] 200 150-300
Platen temperature [oC] 0 0
He flow [sccm] 174 174, 300
C4F8 flow [sccm] 5 5
H2 flow [sccm] 4 0, 4
Pressure [mTorr] 4 2.3, 4

Etch rates in different materials using the standard "Silicon oxide etch with resist mask"

Material to be etched Etch rate using SiO2_res
Thermal oxide ~230nm/min (5% etch load) - etch load dependency see here
TEOS oxide (5% load) 233nm/min ±0.7% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
PECVD1 (standard) oxide (5% load) 242nm/min ±0.6% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
Al2O from the ALD 50nm can be etched in 10min - etched in November 2014 by FRSTO@danchip
Silicon rich nitride from furnace B2 136nm was etched in 1min (whole wafer) - etched in October 2015 by bghe@danchip


Using different resist masks: results using the standard recipe for "Silicon oxide etch with resist mask"

Typical results Test Results Variations over SiO2_res made in 2010 by BGHE See results here
Etch rate of thermal oxide ~230nm/min (5% etch load) - etch load dependency see here ~160-340nm/min
Selectivity to AZ resist [:1] ~3 - etch load dependency [[Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using AOE/AOE SiO2 etch load dependency|see here]| 2.7-4.3
Selectivity to DUV resist [:1] ~2.0 - tested May 2013 by Christian Østergaard @nanotech. ?
Profile [o] ~90 83-90
Images See here See here
Comments A negative resist process was done to make the mask. I have not had so good results with a positive resist process.
Etch rate of TEOS oxide (5% load) 233nm/min ±0.7% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
Etch rate of PECVD1 (standard) oxide (5% load) 242nm/min ±0.6% - "±" represents the non-uniformity over a 100mm wafer - etched in Marts 2013 by LN/BGE@danchip
Etch rate of Al2O from the ALD 50nm can be etched in 10min - etched in November 2014 by FRSTO@danchip
Etch rate of Silicon rich nitride from furnace B2 136nm was etched in 1min (whole wafer) - etched in October 2015 by bghe@danchip
Etch of SiO2 with DUV mask See images here


Striation: Side wall roughness

Slow etch of SiO2 with resist as masking material

Slow etch of SiO2 with resist as masking material - with direct clamping

This recipe can be used for slow etching of SiO2 with resist as masking material when normal clamping is possible. Normal clamping is prefered because it give the best and most repeatable cooling of the wafer. Here are some test results presented.

Parameter Resist mask
Name of Recipe SLOWSIO2
Coil Power [W] 200
Platen Power [W] 25
Platen temperature [oC] 0
CF4 flow [sccm] 20
H2 flow [sccm] 10
Pressure [mTorr] 3


Results Test on maskless wafer Test on wafer with 50% load
Etch rate of thermal oxide 64.9 nm/min (100% etch load) (22-01-2014) 62.8 nm/min (50% etch load) (01-02-2014)
Selectivity to resist [:1] No result ~1.7
Wafer uniformity (100mm) ±0.8% (22-01-2014) ±1.2% (01-02-2014)
Profile [o] Not tested Take a look at the images but be aware that the resist profile was not very good to start with.
Images (click on the image to view a larger image)
Contour plot of the etch rate over the wafer, 5 points measured
Contour plot of the etch rate over the wafer, 9 points measured
SEM images of profile none


Comments . .


Slow etch of SiO2 with resist as masking material - to be used with 150mm Si carrier wafer

The slow etch recipe for oxide etching with photo resist as masking material is called: "slowcool". The recipe has been created to order to be able to have the sample wafer on a si carrier. This means the carrier (150mm with a 102mm recess)is cooled but the wafer on top of it is not. This give a problem with the wafer heating up. The recipe first has a cooling step with no power for 5 min. The etch step parameters and results so fare are as follows:

Parameter Resist mask
Name of recipe SLOWSIO2
Coil Power [W] 200
Platen Power [W] 25
Platen temperature [oC] 0
CF4 flow [sccm] 20
H2 flow [sccm] 10
Pressure [mTorr] 3


Typical results nLOF Resist mask DANCHIP result
Etch rate of thermal oxide 58.5nm/min (50% etch load) (04-09-2013)
Selectivity to nLOF resist [:1] ~1 (04-09-2013)
Wafer uniformity (100mm) ±3.7% (04-09-2013)
Profile [o] ~100degrees (04-09-2013) - probably depends on resist profile
Images (click on the image to view a larger image)


Comments This nLOF negative resist has been used because it can stand more heat in the AOE chamber without getting problems with UV-hardening and evaporation of the solvent leading to a curly resist surface and very rough edges.


Etching of micro structures in Silicon Oxide with PolySi as masking material

The choice of recipe depends on your preferences. Some different etch rate recipes are given here. You can choose between getting


High etch rate recipe

Parameter Recipe name: SiO2_psi (SiO2 etch with pSi mask)
Coil Power [W] 1300
Platen Power [W] 500
Platen temperature [oC] 60
He flow [sccm] 300
C4F8 flow [sccm] 18
H2 flow [sccm] 0
Pressure [mTorr] 4


Typical results PolySi mask - tested by Yunhong Ding @fotonik PolySi mask - tested Feb. 2012 by bge@danchip
Etch rate ~0.55 µm/min 0.50 µm/min
Selectivity 1:~10 1:17
SiO2 etch uniformity not tested ±4.5% over a 100mm wafer
Profile [o] not tested see images
Images . See here
Comments . Line width reduction is about 2.5µm when etching 12.5µm down. See the images to get more info on this


Low line width reduction recipe

It is difficult to get very low line width reduction using P-Si as masiking material. This is due to the fact that the etch gas C4F8 that is used to etch SiO2 also etches Si very well. The best result so fare is given here:

Parameter Poly Si mask
Coil Power [W] 1100
Platen Power [W] 170
Platen temperature [oC] 50
He flow [sccm] 450
C4F8 flow [sccm] 12
H2 flow [sccm] 0
Pressure [mTorr] 6
Spacer settings [mm] 100


Typical results PolySi mask - tested spring. 2012 by bge@danchip
Etch rate ~0.25 µm/min
Selectivity 1:12
SiO2 etch uniformity ±1.1% over a 100mm wafer
Profile [o] see images
Images See here
Comments Line width reduction is about 1µm when etching 7.5µm down. See the images to get more info on this


Good wafer uniformity recipe

This recipe has not been optimized to get as uniformity as possible but was just the one with the lowest non-uniformity among the recipes I have tested.

Parameter Poly Si mask
Coil Power [W] 1300
Platen Power [W] 350
Platen temperature [oC] 60
He flow [sccm] 450
C4F8 flow [sccm] 18
H2 flow [sccm] 7
Pressure [mTorr] 8
Spacer settings [mm] 0


Typical results PolySi mask - tested spring. 2012 by bge@danchip
Etch rate ~0.40 µm/min
Selectivity 1:10
SiO2 etch uniformity (±(max-min/2*avg) ±0.54% over a 100mm wafer
Profile [o] see images
Images See here
Comments Line width reduction is about 3µm when etching 14µm down. See the images to get more info on this


High selectivity to Si-mask recipe

This recipe has not been optimize to get as good selectivity as possible but was just the one with the highest selectivity among the recipes I have tested.


Parameter Poly Si mask
Coil Power [W] 1300
Platen Power [W] 350
Platen temperature [oC] 20
He flow [sccm] 450
CF flow [sccm] 18
H flow [sccm] 7
Pressure [mTorr] 8
Spacer settings [mm] 0


Typical results PolySi mask - tested spring. 2012 by bge@danchip
Etch rate ~0.43 µm/min
Selectivity 1:24
SiO2 etch uniformity ±2.2% over a 100mm wafer
Profile [o] see images
Images See here
Comments Line width reduction is about 3µm when etching 13µm down. See the images to get more info on this


Etching of micro structures in Aluminum oxide

by Fredrik Stöhr

Aluminum oxide (Al2O3, Alumina) can be etched with the standard recipe for silicon oxide etching. The parameters including the chuck temperature are identical to the recipe described above: SiO2_res. The etch is probably very physical and gives redeposition, so please consider using a Cl2 etch on the ICP metal instead (BGHE 2015-04-17)

General Description

Process date: Summer 2014
Aluminum Oxide with a thickness of 50 nm has been deposited by atomic layer deposition using the respective standard recipe.
Substrates: Blank 525 µm Silicon wafers or Silicon wafers with thermally grown Silicon Oxide prior to Alumina deposition.
Mask: [XOP8] AZ5214E 1.5 µm thick (HMDS pretreatment, 6-inch aligner 3 sec exposure, 60 sec development).
Etch Load (Total Exposed SiO2): ~ 5 %
Post process: O2 Plasma Ashing 10 min
Etch time: 3 min. Substrate: Blank Si.
Bird View. The dark area is Silicon. The bright area is Alumina. The black flakes stem from redeposited sputtered material and is most likely aluminum oxide, since it is almost non-volatile in the used plasma chemistry. It must have been laying on top of the photo resist mask and landed on the alumina after resist ashing.
Etch time: 3 min. Substrate: Blank Si.
Bird View. Close-up. The dark area is Silicon. The bright area is Alumina. The black flakes stem from redeposited sputtered material.
Etch time: 3 min. Substrate: Blank Si.
Bird View. Close-up. The dark area is Silicon. The bright area is Alumina.
Etch time: 3 min
Cross section of deep reactive ion etched silicon (DRIE Pegasus), where the structured alumina was used as a mask. Remarkably, the etch selectivity of Alumina to Silicon is >1:10000.
Etch time: 10 min. Substrate: Blank Si.
The view tilt angle is 30°. The edge is corrugated, which is most likely to the corrugated resist mask.
Etch time: 10 min. Substrate: Blank Si.
The view tilt angle is 30°. Vertical striations and considerable over-etching of the Silicon substrate are apparent. It seems as if less material has been redeposited, which may be due to the prolonged etch time in comparison to the above.
Etch time: 10 min. Substrate: Blank Si.
The view tilt angle is 30°. Vertical striations and considerable over-etching of the Silicon substrate are apparent. It seems as if less material has been redeposited, which may be due to the prolonged etch time in comparison to the above.
Etch time: 15 min. Substrate: Silicon with 1 µm thermally grown SiO2
The view tilt angle is 45°. Alumina and Silicon Oxide may be etched in one go.
Etch time: 15 min. Substrate: Silicon with 1 µm thermally grown SiO2
The view tilt angle is 45°. Alumina and Silicon Oxide may be etched in one go. Considerable over-etchign of the Silicon substrate is apparent.
Etch time: 15 min. Substrate: Silicon with 1 µm thermally grown SiO2
The view tilt angle is 45°. Alumina and Silicon Oxide may be etched in one go. Considerable over-etchign of the Silicon substrate is apparent.


Etching with CSAR resist

Information given by Alberto Cagliani February 2015

Using the standard oxide recipe (SiO2_res) for 1 min the CSAR looked burned and could not be removed by CSAR stripper (AR600-71). Using the following settings the resist did not looked burned and could be removed by CSAR stripper:

Parameter Recipe name:
Coil Power [W] 450
Platen Power [W] 80
Platen temperature [oC] 0
He flow [sccm] 174
C4F8 flow [sccm] 5
H2 flow [sccm] 4
Pressure [mTorr] 4


Typical results Negative Resist mask DANCHIP result
Etch rate of thermal oxide ~105nm/min (<5% etch load)
Selectivity to CSAR [:1] ~2
Profile [o] not measured
Images none
Comments CSAR did not burn and could be removed by AR600-71


Limitations using the AOE

Wafer bow

There is a limit to how much the wafer can bow and still be clamped on the chuck. The limit can maybe vary a little over time and may also depend on the material on the backside of the substrate. On a 100mm Si wafer with SiO2 on the backside (<10µm) we expect the limit to be around 50µm bow (when the back side surface is convex).

A bow will be created when etching the top oxide layer on a wafer with oxide on both sides. For a larger etch load the bow will be more severe for a specific etch depth when for a smaller etch load. I have been able to etch much deeper in SiO2 with a P-Si mask than with a photo resist mask on a wafer with 50% load. When using photoresist the wafer stopped clamping during the etch after just a few µm. With P-Si I could etch 15µm without problems. I expect this to be due to a combination of P-Si on the back side clamping much better and P-Si on the back side helping to reduce the bow.


Transparent wafers

Transparent wafers are a challange for two reasons. 1. In the load lock the LASER detection system that is used to detect the wafer during mapping cannot detect a completely transparent wafer. 2. A transparent wafer is either quartz or fused silicon. These materials are very difficult to clamp electrostatically and will therefore not be able to pass the He leak up test succesfully.

  1. The first issue may be overcome by using a non-transparent masking material or adding a non-transparent material on the back side of the wafer (could be aluminium).
  2. The second issue may be overcome by reducing the He back side pressure or reducing the He back side cooling completely. Another way to solve it is to either bond the transparent wafer to a silicon wafer before transfering it into chamber or deposite a more conducting layer on the backside of the wafer. This could be aluminium but also 1-2µm P-Si may be enough.