Thermal evaporation of Aluminum

Aluminum can be thermally evaporated in Wordentec. At DTU Danchip, we recommend to use a thin layer of thermally evaporated aluminum on top of e-beam resist, before the e-beam exposure. For deposition onto the unexposed e-beam resist, you need to use the thermal source.

Recipe

Use process 9 in Wordentec to deposit thermal Aluminum.

Observe: you need to be specially trained to use the thermal deposition source.


Set-up
  • Two "boats" of Tantalum are mounted (on top of each other) in the thermal source each time.
  • If the last deposition from the source was Aluminum, the same boats can be used, otherwise they should be changed.
  • "Small" Al pellets (diameter 1/8", height 1/8") are used. Use these small pellets to get a more uniform deposition with stable deposition rate.
Program settings

Deposition rate is normally 1 or 2 Å/s.

The settings saved in the material file for thermal aluminum are these:

Soak power 1: 5%

Soak power 2: 7%

These are already saved in the process.