Specific Process Knowledge/Thin film deposition/ALD Picosun R200/ZnO deposition using ALD
The ALD window for deposition of zinc oxide (ZnO) ranges from 100 oC to 250 oC. Several investigation techniques has been implemented for ZnO characterization. Additionally, more information on ZnO can be found on a page about Al-doped ZnO (AZO)
All results shown on this page have been obtained using the "ZnOT" recipe on new Si(100) wafers with native oxide:
Al2O3 standard recipe
Recipe: AL2O3
Maximum deposition thickness: 100 nm
Temperature: 100 oC - 350 oC
TMA | H2O | |
---|---|---|
Nitrogen flow | 150 sccm | 200 sccm |
Pulse time | 0.1 s | 0.1 s |
Purge time | 3.0 s | 4.0 s |
This is the standard recipe for deposition of Al2O3 on flat and high aspect ratio structures. For conformal passivation of porous materials, very narrow trenches etc. it is recomanded to use Al2O3T recipe instead. Recipe can be used for deposition in the range 100-350 oC. However, at 100 oC small amount of carbon impurities has been observed. It is not recomanded to use this recipe for deposition below 100 oC, since it also leads to accumulation of H2O in the chamber.
Al2O3 deposition rates
The deposition rate for Al2O3 depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.
In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 100 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.
- Aluminium oxide thickness as function of number of cycles
- Aluminium oxide thickness as function of number of cycles
Evgeniy Shkondin, DTU Danchip, 2014-2016.
Al2O3 standard recipe characterization across 100 mm Si <100> wafer
Al2O3 deposition at 100 oC and 150 oC | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
|
%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
Al2O3 deposition at 200 oC and 250 oC | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
|
%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%
Al2O3 deposition at 300 oC and 350 oC | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
|
Evgeniy Shkondin, DTU Danchip, 2014-2016.
Al2O3 XPS investigation for elemental trace analysis
XPS profile for Al2O3 has been obtained using XPS-ThermoScientific. Al2O3 samples reveals chemically high quality films with no observable contaminations in temperature range 150 - 350 oC. At lower temperature (100 oC) the ALD reaction starts to become unsufficient and some amount of carbon from TMA precursor gets absorbed into the film.
Evgeniy Shkondin, DTU Danchip, 2014-2016.