Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Silicon Nitride Etch using AOE

From LabAdviser

Test of etch in silicon nitride (LPCVD). 105nm nitride had to be removed - it was removed after 1min and 40s with a very small over etch in Si.

Parameter 1Nitride
Coil Power [W] 700
Platen Power [W] 100
Platen temperature [oC] 0
CF flow [sccm] 5
He flow [sccm] 174
H flow [sccm] 4
Pressure [mTorr] 4


Typical results Resist mask
Silicon nitride (LPCVD) etch rate ~60 nm/min 99-108 nm/min (LN/BGE 20130512)
Selectivity to photo resist [:1] ? ~between 2.5 and 4.0 (LN/BGE 20130512)
Etch rate in Si ? ?
Etch rate in SiO2 ? ?
Profile [o] not tested not tested
Images . .
Comments . .