Eutectic bonding
|
Fusion bonding
|
Anodic bonding
|
General description
|
For bonding two substrates by use of an interphase that makes an eutecticum.
|
For bonding two identical materials.
|
For bonding Si and Glass.
|
Bonding temperature
|
Depending on the eutecticum 310 C to 400 C.
|
Depending on defects 50 C to 400 C.
|
Depending on the voltage 300 C to 500 C Standard is 400 C.
|
Annnealing temperature
|
No annealing
|
1000 C in the bond furnace C3
|
No annealing
|
Materials possible to bond
|
Bonding of substrates is done by use of the eutectica Au/Si, Au/Sn and Ni/Si
|
Si/Si, SiO /SiO
|
Si/Pyrex (glass)
|
Substrate size
|
Up to 6" (aligning only possible for 4" and 6")
|
Up to 6" (aligning only possible for 4" and 6")
|
Up to 6" (aligning only possible for 4" and 6")
|
Cleaning
|
Cleaning by N2.
|
Wet chemical cleaning, IMEC.
|
Cleaning by N2.
|