Specific Process Knowledge/Etch/Etching of Silicon/Si etch using RIE1 or RIE2/Specific Process Knowledge/Etch/Etching of Silicon/Si etch using RIE1 or RIE2/RIE1 Travka results: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
Line 1: Line 1:
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=


=== RIE1 Travka results - Etch rate and profile as function of etch load===
=== RIE1 Travka results - Silicon etch rate and profile as function of etch load===
 
<b>Purpose</b>
 
The purpose of the RIE1 Travka experiments is the measure the silicon etch rate and profile as function fo the etch load, i.e. the percentage of the wafer that is etched.
 
<b>Experiment</b>


Seven silicon wafers have been etched in RIE1 using the "OH_polyA" recipe.
Seven silicon wafers have been etched in RIE1 using the "OH_polyA" recipe.


All wafers have the same resist pattern ("Travka" masks), but the etch load is differs from wafer to wafer. For more information about the "Travka" masks see xxx.
All wafers have the same resist pattern ("Travka" masks), but the etch load is differs from wafer to wafer. For more information about the "Travka" masks see xxx.
The wafers have been etched in June 2012.
<b>Measurements </b>


After the etching the wafers have been cleaved, and trechnes with different mask widths have been inspected with SEM in order to measure resist etch rate, the Si etch depth, the under etch and the trench width. From the Si etch depth the Si etch rate has been calculated.  
After the etching the wafers have been cleaved, and trechnes with different mask widths have been inspected with SEM in order to measure resist etch rate, the Si etch depth, the under etch and the trench width. From the Si etch depth the Si etch rate has been calculated.  


The resist thickness has been measured on the Filmtek before and after the RIE etching, and thus the resist etch rate is calculted.  
The resist thickness has been measured on the Filmtek before and after the RIE etching, and thus the resist etch rate is calculted.  


The results of the RIE etching, including SEM images of the etching profiles, are show below.
The results of the RIE etching, including SEM images of the etching profiles, are show below.
The wafers have been etched June 2012.


==Process flow and parameters==
==Process flow and parameters==

Revision as of 11:44, 3 April 2013

THIS PAGE IS UNDER CONSTRUCTIONUnder construction.png

RIE1 Travka results - Silicon etch rate and profile as function of etch load

Purpose

The purpose of the RIE1 Travka experiments is the measure the silicon etch rate and profile as function fo the etch load, i.e. the percentage of the wafer that is etched.

Experiment

Seven silicon wafers have been etched in RIE1 using the "OH_polyA" recipe.

All wafers have the same resist pattern ("Travka" masks), but the etch load is differs from wafer to wafer. For more information about the "Travka" masks see xxx.

The wafers have been etched in June 2012.

Measurements

After the etching the wafers have been cleaved, and trechnes with different mask widths have been inspected with SEM in order to measure resist etch rate, the Si etch depth, the under etch and the trench width. From the Si etch depth the Si etch rate has been calculated.

The resist thickness has been measured on the Filmtek before and after the RIE etching, and thus the resist etch rate is calculted.


The results of the RIE etching, including SEM images of the etching profiles, are show below.

Process flow and parameters

Photolithography Resist thickness
  • 1.5 µm
Resist masks and etch loads
  • "Travka5", etch load 5%
  • "Travka10", etch load 10%
  • "Travka20", etch load 20%
  • "Travka35", etch load 35%
  • "Travka50", etch load 50%
  • "Travka65", etch load 65%
  • "Travka80", etch load 80%
Measure resist thickness Filmtek parameters
  • Recipe: "RIE_Travka_2points"
  • Points: (x,y) = (10,10);(-10,-10)
RIE preconditioning Before preconditioning
  • Check that the "Clean20" recipe has been run
RIE1 preconditioning parameters
  • Wafer: dummy wafer
  • Recipe: "RIETrav" (same settings as the "OH_polyA" recipe)
  • Time: 8 minutes
RIE etching Before etching
  • Move native oxide in BHF
RIE1 etching parameters
  • Recipe: Recipe: "RIETrav2 (same settings as the "OH_polyA" recipe)
  • Time: 8 minutes
Note
  • Etch all wafers the same day
Measure resist thickness Filmtek parameters
  • Recipe: "RIE_Travka_2points"
  • Points: (x,y) = (10,10);(-10,-10)
SEM characterization Note
  • Cleave wafers at ARDE lines (lower right corner towards the flat)
Mask trench widths to be measured
  • 2 µm
  • 4 µm
  • 10 µm
  • 50 µm
  • 200 µm
Measurements
  • Trench width
  • Si etch depth
  • Si etch angle
  • Underetch


Results

Silicon etch rate as function



A table with the etching result can be found here:

xxx

Mask Resist etch rate [nm/min] Silicon etch rate [µm/min] Trench width [µm] Under etch [µm] Silicon etch angle [oC]
2 µm 4 µm 10 µm 50 µm 200 µm 2 µm 4 µm 10 µm 50 µm 200 µm 2 µm 4 µm 10 µm 50 µm 200 µm 2 µm 4 µm 10 µm 50 µm 200 µm
Travka5 67.31 0.6 0.63 0.63 0.62 0.61 2.60 4,91 10.96 51.00 201.90
Travka10 63.94 0.57 0.59 0.59 0.58 0.61 2.32 4.60
Travka20 63.13 0.63 0.63 0.64 0.64 0.59
Travka35 59.63 0.57 0.60 0.61 0.61 0.55
Travka50 57.13 0.47 0.5 0.51 0.51 0.49
Travka65 57.88 0.41 0.41 0.42 0.42 0.43
Travka80 57.56 0.37 0.36 0.37 0.37 0.38
Common Temperature 20 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers