(New page: RIE (Reactive Ion Etch) can be used for etching silicon oxide. The etch is anisotropic with vertical or angled sidewalls depending on the process recipe and the masking material and geomet...)
 
Line 13: Line 13:
*Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
*Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)


==Most used recipe (this recipe is being watched in the in the quality assurance program):==
==Most used recipes:==


===Resist as masking material:===
{| border="1" cellspacing="1" cellpadding="2"  align="left"
{| border="1" cellspacing="1" cellpadding="2"  align="left"
! Recipe:
! Recipe:
! 1SiO2mre
! 1SiO2mre
|-  
|-  
|Masking material
|Photoresist
|-
| CF<sub>4</sub> flow
| CF<sub>4</sub> flow
|14 sccm
|14 sccm
Line 50: Line 54:
|~30 nm/min
|~30 nm/min
|-
|-
|Etch rate in Si (when not etching SiO2 at the same time)
|Etch rate in Si
(etching down to Si)
|Expected <2 nm/min
|Expected <2 nm/min
|Expected <2 nm/min
|Expected <2 nm/min
Line 56: Line 61:
|}
|}
mre:mask resist
mre:mask resist
===PolySilicon as masking material===
{| border="1" cellspacing="1" cellpadding="2"  align="left"
! Recipe:
! 1SiO2msi
|-
|Masking material
|Silicon
|-
| CF<sub>4</sub> flow
|8 sccm
|-
|CHF<sub>3</sub> flow
|40 sccm
|-
|Pressure
|150 mTorr
|-
|RF-power
|150 W
|-
|}
{| border="2" cellspacing="1" cellpadding="3" align="center"
!
!Expected results in RIE1
!Expected results in RIE2
|-
|Etch rate in SiO<sub>2</sub>
|~70-80 nm/min
|~70-80 nm/min
|-
|Etch rate in Si<sub>3</sub>N<sub>4</sub>
|?
|?
|-
|Etch rate in P-Si (when used as mask)
|~20-30 nm/min
|~20-30 nm/min
|-
|Etch rate in Si
(etching down to Si)
|?
|?
|-
|}
msi:mask silicon
===Burned resist as masking material (developed for waveguides):===
{| border="1" cellspacing="1" cellpadding="2"  align="left"
! Recipe:
! 1SiO2mbr
|-
|Masking material
|Burned resist (250<sub>o</sub>C)
|-
|CHF<sub>3</sub> flow
|84 sccm
|-
|Pressure
|60 mTorr
|-
|RF-power
|200 W
|-
|}
{| border="2" cellspacing="1" cellpadding="3" align="center"
!
!Expected results in RIE1
!Expected results in RIE2
|-
|Etch rate in SiO<sub>2</sub>
|~120 nm/min
|~120 nm/min
|-
|Etch rate burned resist
|?
|?
|-
|Etch rate in Si<sub>3</sub>N<sub>4</sub>
|?
|?
|-
|Etch rate in P-Si (when used as mask)
|? nm/min
|? nm/min
|-
|Etch rate in Si
(etching down to Si)
|?
|?
|-
|}
mbr:mask burned resist

Revision as of 13:14, 13 November 2007

RIE (Reactive Ion Etch) can be used for etching silicon oxide. The etch is anisotropic with vertical or angled sidewalls depending on the process recipe and the masking material and geometry. The SiO2 is etched by flour radicals assisted by ion bombardment.

The substrate:

Most be a wafer of 4" or below or small pieces, not higher than about 2mm.

The silicon can be masked by these materials:

  • Photoresist
  • E-beam resist
  • Silicon
  • Silicon Nitride
  • Aluminium
  • Chromium (ONLY RIE2!)
  • Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)

Most used recipes:

Resist as masking material:

Recipe: 1SiO2mre
Masking material Photoresist
CF4 flow 14 sccm
CHF3 flow 26 sccm
Pressure 100 mTorr
RF-power 60 W
Expected results in RIE1 Expected results in RIE2
Etch rate in SiO2 ~20-30 nm/min ~20-30 nm/min
Etch rate in Si3N4 ? ?
Etch rate in P-Si (when used as mask) ~30 nm/min ~30 nm/min
Etch rate in Si

(etching down to Si)

Expected <2 nm/min Expected <2 nm/min

mre:mask resist

PolySilicon as masking material

Recipe: 1SiO2msi
Masking material Silicon
CF4 flow 8 sccm
CHF3 flow 40 sccm
Pressure 150 mTorr
RF-power 150 W
Expected results in RIE1 Expected results in RIE2
Etch rate in SiO2 ~70-80 nm/min ~70-80 nm/min
Etch rate in Si3N4 ? ?
Etch rate in P-Si (when used as mask) ~20-30 nm/min ~20-30 nm/min
Etch rate in Si

(etching down to Si)

? ?

msi:mask silicon

Burned resist as masking material (developed for waveguides):

Recipe: 1SiO2mbr
Masking material Burned resist (250oC)
CHF3 flow 84 sccm
Pressure 60 mTorr
RF-power 200 W
Expected results in RIE1 Expected results in RIE2
Etch rate in SiO2 ~120 nm/min ~120 nm/min
Etch rate burned resist ? ?
Etch rate in Si3N4 ? ?
Etch rate in P-Si (when used as mask) ? nm/min ? nm/min
Etch rate in Si

(etching down to Si)

? ?

mbr:mask burned resist