Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using ASE/ICP recipe for SiO2: Difference between revisions
Jump to navigation
Jump to search
Line 40: | Line 40: | ||
|155 nm/min in the center, 125nm/min in the edges | |155 nm/min in the center, 125nm/min in the edges | ||
(03052023 mfarin @ DTU nanolab) | (03052023 mfarin @ DTU nanolab) | ||
| | |||
| | | | ||
| | | | ||
Line 46: | Line 47: | ||
|108 nm/min in the center, 98nm/min in the edges | |108 nm/min in the center, 98nm/min in the edges | ||
(03052023 mfarin @ DTU nanolab) | (03052023 mfarin @ DTU nanolab) | ||
| | |||
| | |||
| | | | ||
|- | |- | ||
|Selectivity (SiO2:resist) | |Selectivity (SiO2:resist) | ||
|1.45 | |1.45 | ||
| | |||
| | |||
| | | | ||
|- | |- | ||
|Etch rate in silicon | |Etch rate in silicon | ||
| | |||
| | |||
| | | | ||
| | | |
Revision as of 09:54, 24 May 2023
This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.
Parameter | Recipe name: SiO2_ICP |
---|---|
Coil Power [W] | 1000 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
C4F8 flow [sccm] | 10 |
H2 flow [sccm] | 28 |
Pressure [mTorr] | 2.5 |
Results when etching a patterned wafer