|Etch rate in SiO2
|Etch rate in SiO2
|155 nm/min in the center, 125nm/min in the edges (03052023 mfarin @ DTU nanolab)
|155 nm/min in the center, 125nm/min in the edges
(03052023 mfarin @ DTU nanolab)
|
|
|-
|-
|Etch rate in resist (AZ 5214E)
|Etch rate in resist (AZ 5214E)
|108 nm/min in the center, 98nm/min in the edges (03052023 mfarin @ DTU nanolab)
|108 nm/min in the center, 98nm/min in the edges
(03052023 mfarin @ DTU nanolab)
|
|
|-
|-

Revision as of 09:53, 24 May 2023

This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.


Parameter Recipe name: SiO2_ICP
Coil Power [W] 1000
Platen Power [W] 200
Platen temperature [oC] 20
C4F8 flow [sccm] 10
H2 flow [sccm] 28
Pressure [mTorr] 2.5

Results when etching a patterned wafer

Material to be etched Recipe: SIO2_ICP SIO2_ICP on stoic Nit SIO2_ICP on low-stress Nit SIO2_ICP on Si
Etch rate in SiO2 155 nm/min in the center, 125nm/min in the edges

(03052023 mfarin @ DTU nanolab)

Etch rate in resist (AZ 5214E) 108 nm/min in the center, 98nm/min in the edges

(03052023 mfarin @ DTU nanolab)

Selectivity (SiO2:resist) 1.45
Etch rate in silicon
Profile Images SiO2 ICP.2-top-02.png