Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using ASE/ICP recipe for SiO2: Difference between revisions
Jump to navigation
Jump to search
Tag: Manual revert |
|||
Line 33: | Line 33: | ||
!Material to be etched | !Material to be etched | ||
!Recipe: SIO2_ICP | !Recipe: SIO2_ICP | ||
! | !SIO"_ICP on stoic Nit | ||
!SIO"_ICP on Nit | |||
!SIO"_ICP on stoic Nit | |||
|- | |- | ||
|Etch rate in SiO2 | |Etch rate in SiO2 |
Revision as of 09:51, 24 May 2023
This recipe was taken from the ICP Metal etch, with a slight difference in the platen temperature.
Parameter | Recipe name: SiO2_ICP |
---|---|
Coil Power [W] | 1000 |
Platen Power [W] | 200 |
Platen temperature [oC] | 20 |
C4F8 flow [sccm] | 10 |
H2 flow [sccm] | 28 |
Pressure [mTorr] | 2.5 |
Results when etching a patterned wafer