Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)/AlN deposition using ALD2/Acceptance test AlN: Difference between revisions
Created page with "==AlN with N<sub>2</sub> plasma== <!-- Experiment 161102A --> The test was done with 300 cycles at 350 °C where the growth rate was measured to be '''0.0625 nm/cycle'''. ..." |
No edit summary |
||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/LabAdviser/Courses/TPT_Thin_Film click here]''' | |||
''This page is written by DTU Nanolab internal'' | |||
==AlN with N<sub>2</sub> plasma== <!-- Experiment 161102A --> | ==AlN with N<sub>2</sub> plasma== <!-- Experiment 161102A --> | ||
The test was done with 300 cycles at 350 °C where the growth rate was measured to be '''0.0625 nm/cycle'''. | The test was done with 300 cycles at 350 °C where the growth rate was measured to be '''0.0625 nm/cycle'''. |
Revision as of 09:58, 10 May 2023
Feedback to this page: click here
This page is written by DTU Nanolab internal
AlN with N2 plasma
The test was done with 300 cycles at 350 °C where the growth rate was measured to be 0.0625 nm/cycle.
TMA | N2 plasma | |
---|---|---|
Nitrogen flow | 150 sccm | 100 sccm |
Pulse time | 0.1 s | 21.0 s |
Purge time | 4.0 s | 4.0 s |
Uniformity profile across 150 mm Si wafer based on 49 measurement points measured with ellipsometer. The values for the grown oxide thickness can be seen in the table below.
Parameter | Average | Min. | Max. | Std.Dev | %Range |
---|---|---|---|---|---|
Thickness (nm) | 18.77 | 18.02 | 19.73 | 0.41 | 9.0619 |
Pernille Voss Larsen, Mikkel Dysseholm Mar and Tanja Amport, DTU Nanolab, 2016-2017.
AlN with N2 plasma on trenches
The test was done with 1000 cycles at 350 °C.
TMA | N2 plasma | |
---|---|---|
Nitrogen flow | 150 sccm | 100 sccm |
Pulse time | 0.1 s | 26.0 s |
Purge time | 4.0 s | 15.0 s |
Additionally the picoflow was used for the TMA precursor.
As the SEM images above show only a thin layer of AlN could be deposited at the bottom of the trenches. On the top the growth was significantly higher which lead to a tree like growth. Whereas in the images below no picoflow was used with 500 cycles and the same other parameters as in the run shown above. Without the picoflow a more homogeneous coverage could be obtained and an average growth rate of 0,05585 nm/cycle was measured.
Pernille Voss Larsen, Mikkel Dysseholm Mar and Tanja Amport, DTU Nanolab, 2016-2017.