Specific Process Knowledge/Thin film deposition/Deposition of Silicon Nitride/Deposition of silicon nitride using Lesker sputter system: Difference between revisions

From LabAdviser
Jump to navigation Jump to search
(added more info on new cluster sputter system chambers with links)
Line 32: Line 32:
|4
|4
|10
|10
|Ar+45%N2
|N2 ratio 45% (Ar:33 sccm + N2: 15 sccm)
|RT
|RT
|~1.7nm/min  
|~1.38 nm/min  
|-
|-
|source 1 DC with RF bias and nitrogen
|source 1 DC with RF bias and nitrogen

Revision as of 10:33, 30 August 2022

Feedback to this page: click here


The sputter-system(Lesker) can be use to deposit silicon nitride by reactive sputtering with a gas mixture of Ar and N2, where N2 is the reactive gas.

We have little experience with this so any information you obtain will be welcome.

Note that it is also possible to deposit SiN by reactive sputtering in the newer Sputter-System Metal-Nitride(PC3) which is a dedicated chamber for metal and nitride deposition where oxygen contamination of the film will be minimized. SiOxNy may be deposited in Sputter-System Metal-Oxide(PC1). These chambers also offer pulsed DC sputtering and HIPIMS (high-power impulse magnetron sputtering).


Recipes on Sputter-System(Lesker) for deposition of silicon nitride

Recipes

The recipe below has been tried in the system. It is possible to change many of the parameters.

Recipe name Target Gun Power [W] Pressure [mTorr] RF substrate Power [W] Gas Temperature Deposition rate
source 3 DC with nitrogen Si 3 90 4 10 N2 ratio 45% (Ar:33 sccm + N2: 15 sccm) RT ~1.38 nm/min
source 1 DC with RF bias and nitrogen Si 1 180 4 No Ar+45%N2 RT ~4.25nm/min